A method for purifying and whitening phosphogypsum

Through flotation, high-speed centrifugal dehydration and segmented temperature-controlled electromagnetic rotary furnace processing, combined with ultra-fine grinding, the problems of low efficiency and high energy consumption in the purification and whitening of phosphogypsum are solved, and high-purity, high-whiteness sulfuric acid is achieved. Calcium powder production for a variety of industrial applications.

CN116116885BActive Publication Date: 2024-10-18HUNAN ZHENYA NEW MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211383095.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-03
Publication Date
2024-10-18
Estimated Expiration
2042-11-03

AI Technical Summary

Technical Problem

The existing technology cannot effectively purify and whiten phosphogypsum, resulting in its insufficient purity and whiteness in industrial applications and its inability to meet higher requirements for use in fields. The treatment process has low efficiency, high energy consumption, high cost, and cannot be completely removed. Removal of crystallized water affects product quality.

Method used

The phosphogypsum powder is flotated using a composite flotation agent, and then dehydrated in a high-speed centrifugal dehydrator, and then dried, desorbed water and crystal water through a segmented temperature-controlled electromagnetic rotary furnace, and finally rapidly cooled in a rotary cooling furnace , obtain anhydrous calcium sulfate powder, and grind it finely in an ultra-fine mill to obtain high-performance filler.

Benefits of technology

It achieves low-carbon, environmentally friendly, energy-saving, low-cost purification and whitening of phosphogypsum. The purity of the product is as high as over 95%, and the whiteness is as high as over 88%. Crystal water and impurities are removed, and the weather resistance and dispersion of the product are improved. It is suitable for Various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003924007280000081
    Figure BDA0003924007280000081
  • Figure BDA0003924007280000082
    Figure BDA0003924007280000082
  • Figure BDA0003924007280000091
    Figure BDA0003924007280000091
Patent Text Reader

Abstract

A method for purifying and whitening phosphogypsum includes the following steps: (1) mixing solid waste phosphogypsum powder with water to form a mixed slurry, and then adding a flotation agent for flotation; (2) placing the phosphogypsum mixed slurry obtained by flotation in a high-speed centrifugal dewatering machine for centrifugal dewatering to obtain phosphogypsum powder with a water content of less than 15%; (3) feeding the phosphogypsum powder into an electromagnetic rotary furnace for preheating, drying, dewatering, stepwise decrystallization, and calcination, with the temperature gradually increasing to obtain phosphogypsum powder with a temperature below 360℃; (4) feeding the phosphogypsum powder with a temperature below 360℃ into a rotary cooling furnace for rapid cooling; (5) feeding the obtained calcium sulfate powder into an ultrafine grinding mill for fine grinding to obtain calcium sulfate powder that can be used as a high-performance filler. This invention is low-carbon and environmentally friendly, with low energy consumption and low processing cost. The obtained product has high purity and high whiteness and can be used as a filler for the production of films and plastics. The films and plastic products made from it have good antioxidant and UV resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for treating industrial waste slag phosphogypsum, in particular to a method for purifying and whitening industrial waste slag phosphogypsum generated in the production of phosphate fertilizer. Background Art

[0002] As a common inorganic substance, gypsum is favored in various fields such as building materials, medicine and food, paint and coating, aerospace, and plastics, and has a wide range of applications. With the rapid development of social economy, the demand for gypsum is increasing, and at the same time, higher requirements are placed on the quality of gypsum.

[0003] Phosphogypsum refers to the solid waste residue produced when phosphate ore is treated with sulfuric acid during the production of phosphate fertilizer using phosphate ore as raw material. Every ton of phosphate fertilizer produced will produce 4.5 tons of phosphogypsum. The main component of phosphogypsum is calcium sulfate dihydrate (molecular formula CaSO4·2H2O). Phosphogypsum contains a large amount of impurities, such as SiO2, insoluble P2O5, eutectic P2O5, F, AL2O3, MgO and other 27 heavy metals and fluorides and sulfates, which make phosphogypsum cannot be directly used in the field of building materials, let alone in other fields with higher requirements. It becomes industrial solid waste, which not only occupies land but also pollutes the environment. The current stockpile of phosphogypsum exceeds 820 million tons, and the annual increase is more than 78 million tons. The treatment of phosphogypsum has become a difficulty and pain point in the current national environmental governance.

[0004] CN111377632A discloses a phosphogypsum treating agent, a phosphogypsum treating method, a phosphogypsum filling material preparation method and a phosphogypsum filling material. The phosphogypsum treating method first uses calcined 27.7%-96.7% phosphate tailings, adds 0.3%-1% ammonium sulfate, 0-3.5% alkaline activator, and 3%-68% solid waste fine powder to prepare a phosphogypsum treating agent. When treating newly produced phosphogypsum, 3%-8% of the treating agent is directly added to the phosphogypsum slurry for stirring; when treating phosphogypsum that has been stored for a period of time, since the phosphogypsum has been stored in blocks, the treating agent needs to be prepared into a suspension with a concentration of 30%-60% and sprayed on the surface of the phosphogypsum, and then the pile is turned over and sprayed again, and this process is repeated several times to passivate the soluble harmful substances in the phosphogypsum, thereby reducing the harmfulness of the phosphogypsum. The biggest advantage of this phosphogypsum treatment method is that it treats solid waste with solid waste. The disadvantage is that it does not involve the purification and whitening of phosphogypsum, nor does it involve the removal of harmful substances in phosphogypsum. It only passivates the harmfulness of phosphogypsum by adding gypsum treatment agents and reduces the diffusion of harmful substances in phosphogypsum. The phosphogypsum treated by this method has no comprehensive utilization value and can only be used as a filling material for mine closure.

[0005] CN105524325A discloses a new method for utilizing phosphogypsum. The steps are as follows: (1) drying the phosphogypsum at 150-180°C for 5-25min, and then directly calcining the phosphogypsum at 500-600°C for 1-2min to form modified phosphogypsum; (2) mixing the modified phosphogypsum with polyethylene in a ratio of 10-85:15-90 to form a mixture and sending it to a mixer for granulation; then sending it to a calender for extrusion and stretching to form a 0.02-2mm film. The phosphogypsum treated by this technology is not scientifically set due to the calcination temperature and time, which is not only difficult to remove the crystal water in the phosphogypsum, but also the attached water will be higher than the national standard of 3‰; the treatment method does not involve the purification and whitening of phosphogypsum. The phosphogypsum treated by this method cannot be used as a filling material, and its application range is limited; it is applied to the production of film materials, and the quality of the obtained film materials is worrying.

[0006] CN105330966A discloses a method for producing PP materials using phosphogypsum as filler. The steps are as follows: (1) frying the phosphogypsum in a wok at 150-200°C for 20-30 minutes, grinding it and then grading and screening it, and then using a vibrating screen to grade and remove impurities from the powder, and grading out phosphogypsum powder with a particle size of no more than 10um; (2) mixing titanium dioxide, water and phosphogypsum powder, sending them into a mill, grinding them into a powder of 300-800 mesh, and then transferring the powder into an aging tank and stirring it for 10-20 minutes, introducing carbon dioxide gas, and the temperature of the high-speed aging tank is 80-150°C. Stir and react for 20-40 minutes, then add nano silicon dioxide, which is 1-3 times the weight of titanium dioxide, stir for 5-10 minutes, grind into 300-800 mesh powder, stir at 150-200°C for 50-60 minutes to obtain the initial material; (3) add the material to PP at a ratio of 20-30% of the weight of PP, stir in a high-speed stirring mixer for 20-30 minutes, and extrude through a twin-screw extruder at 210°C. The disadvantages of this technology are that repeated frying, repeated stirring, repeated grinding, long time, low efficiency, high energy consumption, high processing cost, no purification of phosphogypsum, only use titanium dioxide to change the whiteness of phosphogypsum, and the improvement of the whiteness of phosphogypsum is limited. In addition, studies have shown that under temperature conditions of 150-200°C, the crystal water in phosphogypsum cannot be completely removed to become anhydrous gypsum. In actual production, the phosphogypsum powder obtained by this method is used as a filling material for producing PP, and the quality of the resulting PP product is difficult to guarantee.

[0007] CN105331009A discloses a powdered phosphogypsum filler and a preparation method thereof, comprising the following steps: sintering the phosphogypsum to a surface temperature of 180-190°C, grinding to a particle size of 60-80um to obtain β-type hemihydrate gypsum, adding an additive and a dispersant, mixing at high speed for 5-8min, maintaining at a constant temperature of 60-90°C for 30-60min, and grinding into powder to obtain a powdered phosphogypsum filler. The dispersant is a mixture of one or more of paraffin, citrate, stearate, polypropylene wax, and polyethylene wax. The disadvantage of this technology is that a high-temperature mill is required, which has low efficiency and high energy consumption, does not remove impurities and harmful substances in the phosphogypsum, and does not improve the purity and whiteness of the phosphogypsum. The phosphogypsum powder treated by this technology has a limited application range and can only be used as a filling material for paper-faced gypsum boards. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the above-mentioned defects existing in the prior art and provide a method for purifying and whitening phosphogypsum which is low-carbon, environmentally friendly, low-energy consumption, low processing cost, and has a high purity and high whiteness of the obtained product.

[0009] The technical solution adopted by the present invention to solve the technical problem is a method for purifying and whitening phosphogypsum, comprising the following steps:

[0010] (1) preparing a mixed slurry of industrial solid waste phosphogypsum powder and water, and then adding a composite flotation agent to the phosphogypsum mixed slurry for flotation to obtain a phosphogypsum mixed slurry from which impurities have been preliminarily removed;

[0011] (2) placing the phosphogypsum mixed slurry obtained in step (1) in a high-speed centrifugal dehydrator for centrifugal dehydration to obtain a hydrated phosphogypsum powder having a water content of less than 15%;

[0012] (3) feeding the hydrated phosphogypsum powder obtained in step (2) into an electromagnetic rotary furnace, and sequentially performing preheating, drying, desorption of attached water, stepwise desorption of crystallization water, and calcination through staged temperature control, and gradually increasing the temperature to sequentially remove attached water, crystallization water, and residual impurities not removed in the flotation process of step (1) in the hydrated phosphogypsum powder, thereby obtaining phosphogypsum powder with a temperature of less than 360° C.;

[0013] (4) feeding the phosphogypsum powder obtained in step (3) at a temperature below 360° C. into a rotary cooling furnace and rapidly cooling the powder to room temperature through water circulation to obtain calcium sulfate powder;

[0014] (5) The calcium sulfate powder obtained in step (4) is fed into an ultrafine grinding machine for fine grinding to obtain calcium sulfate powder with an average particle size of 1200-6000 mesh that can be used as a high-performance filler.

[0015] If the product is used as a building material, step (5) can be omitted.

[0016] Furthermore, in step (1), the particle size of the phosphogypsum powder is 200-350 mesh, preferably 250-300 mesh. When the particle size is less than 350 mesh, the centrifugal dehydration efficiency is reduced, and when the particle size is greater than 250 mesh, the flotation effect is poor.

[0017] Furthermore, in step (1), in the phosphogypsum mixed slurry, the phosphogypsum powder accounts for 25-35wt%; preferably 28-32wt%, more preferably 30wt%; water accounts for 65-75wt%, preferably 70wt%. Multiple tests have shown that this ratio has the best flotation cost-effectiveness, the best flotation effect, and the most energy saving.

[0018] Furthermore, in step (1), the composite flotation agent is prepared by mixing polyoxybutylene alcohol dithiophosphate and alkyl dithiocarbonate. The flotation agent has a better flotation effect and is cheaper.

[0019] Furthermore, in the composite flotation agent, the weight ratio of the polyoxybutylene alcohol dithiophosphate to the hydrocarbon dithiocarbonate is 1-5: 1, preferably 3-4: 1. The specific ratio is determined according to the difference in impurity content between phosphogypsum and other industrial gypsum.

[0020] Furthermore, in step (1), the addition amount of the composite flotation agent is 0.01%-0.05% by weight of the phosphogypsum mixed slurry, preferably 0.03%-0.05%.

[0021] Furthermore, in step (1), the flotation is column classification flotation, which is convenient for sequentially removing heavy metals and other impurities of different specific gravities.

[0022] Furthermore, in step (2), the rotation speed of the high-speed centrifuge is 8000r / min-30000r / min, preferably 20000r / min-25000r / min; this rotation speed is highly efficient and energy-saving, and can increase production capacity under homogeneous conditions.

[0023] Furthermore, in step (3), the drying and dehydration method is electromagnetic rotary furnace drying.

[0024] Furthermore, in step (3), the segmented temperature control is as follows: preheating temperature 80°C-100°C; drying temperature 120°C-150°C; decrystallization water and impurity removal temperature 220°C-360°C. The first temperature control zone (preheating temperature control zone) is set to 80°C-100°C, the second temperature control zone (drying and deattaching water temperature control zone) is set to 120°C-150°C, the third to fifth temperature control zones (stepwise decrystallization water temperature control zones) are set to 220°C-320°C, and the sixth temperature control zone (impurity removal temperature control zone) is set to 300°C-360°C.

[0025] If the product is used as a building material, due to the low requirement for impurity content, in order to save energy, the temperature of the 6th temperature control zone (impurity removal temperature control zone) can be set below 250℃, 220℃-250℃.

[0026] Furthermore, in step (3), the time control of each section is as follows: the first temperature control zone: preheating time is 10min-15min; the second temperature control zone: drying time is 20min-25min; the third to sixth temperature control zones, the time for removing crystallized water and burning to remove impurities is 30min-40min, and the total time for preheating, drying to remove attached water, removing crystallized water, and burning to remove impurities is controlled to be 0.9h-1.5h, preferably 1h-1.2h.

[0027] Furthermore, in step (5), the ultrafine grinder is a roller mill.

[0028] In step (5), the specific selection of the particle size of the finely ground product should be determined according to the specific application. For example, for use as a plastic filler, an average particle size of 1250 mesh is preferred; for use as a film filler, an average particle size of 2000 mesh is preferred; and for use as a high-grade paint filler, an average particle size of 6000 mesh is preferred.

[0029] Studies have shown that drying to remove attached water, crystallization water and impurities uses a traditional pulverized coal furnace or natural gas furnace. The coal or natural gas is sprayed into the furnace mouth for combustion, and the gypsum powder is released from the furnace tail. During the entire heating process, the temperature in the furnace tends to gradually decrease, which cannot achieve the purpose of completely removing crystallization water and impurities. In addition, the temperature is not easy to control and master, and the energy consumption is high, the production cost is high, and there is carbon dioxide gas emission, which affects the environmental protection. In particular, the temperature of the wet phosphogypsum material should be gradually increased from preheating to removing attached water, crystallization water and burning to remove impurities, rather than gradually decreasing. Moreover, the removal of crystallization water should be carried out in steps using different temperatures so that the crystallization water can be completely removed and the impurities can be basically removed, thereby achieving the expected effect. The present invention sets a flotation process (preferably a column classification flotation process) before heating and dehydrating the phosphogypsum to remove most of the main impurities therein, and then uses a segmented automatic temperature-controlled electromagnetic rotary furnace to replace the traditional pulverized coal furnace or natural gas cooking furnace or boiling furnace, and controls the phosphogypsum wet material obtained by flotation from preheating to desorption of attached water, step-by-step desorption of crystallization water, and calcination to remove impurities, and the temperature gradually increases rather than gradually decreases, thereby obtaining anhydrous calcium sulfate powder with complete desorption of crystallization water, extremely low impurity content, high purity, and white color. The inventors also found that the temperature of crystallization water in dephosphogypsum is not the higher the better. If the temperature is too high, not only energy is wasted, but also the crystallization water is not completely removed. The maximum temperature for desorption of crystallization water should not exceed 320°C. The present invention uses an automatic temperature-controlled electromagnetic rotary furnace to dry and desorption of attached water, step-by-step desorption of crystallization water, and calcination to remove impurities from the phosphogypsum wet material obtained by flotation, which completely overcomes the shortcomings of pulverized coal furnaces or natural gas furnaces, is convenient for temperature control, has low energy consumption, no carbon emissions, and no pollution. It is an ideal low-carbon, energy-saving and environmentally friendly production method. The preferred solution is to use the column classification flotation method to make the phosphogypsum slurry pass through different column flotation barrels in turn. Under the action of the flotation agent, the impurities of different specific gravities are selected one by one through stirring and floating. This is the most advanced non-metallic mineral powder flotation method. The waste silicon material produced by flotation can be used to burn cement or as a building material after natural drying; the waste oil carbon produced by flotation can be used as fuel; the waste barium material produced by flotation can be used to produce industrial barium oxide for glass and ceramic product manufacturing, or as a dehydration desiccant; the water can be recycled after sedimentation.

[0030] In summary, the phosphogypsum purification and whitening treatment method of the present invention is low-carbon, environmentally friendly, energy-saving, and has no secondary pollution; the treatment cost is low; the obtained product has a small impurity content, a purity of more than 95%, a whiteness of more than 88, and does not contain crystal water. The calcium sulfate powder produced by the phosphogypsum purification and whitening method of the present invention has good weather resistance, corrosion resistance, and good dispersibility through test comparison with heavy calcium, talcum powder, calcium carbonate powder, and barium sulfate powder. It is used as a filler for producing thin films. The prepared thin films have high transparency and good antioxidant and UV resistance. DETAILED DESCRIPTION

[0031] The present invention is further described below with reference to the embodiments.

[0032] The electromagnetic rotary furnace used in each embodiment was purchased from Hunan Qijiexin Electronic Technology Co., Ltd.; polyoxybutylene alcohol dithiophosphate and alkyl dithiocarbonate were purchased from Zhuzhou Mingzhu Mineral Processing Reagent Co., Ltd.; and the column flotation equipment was purchased from Hunan Zhonggong Mining Engineering Technology Co., Ltd.

[0033] Example 1

[0034] (1) 300-mesh phosphogypsum powder and water are mixed into a phosphogypsum mixed slurry in which water accounts for 70wt% and phosphogypsum powder accounts for 30wt%, a composite flotation agent of polyoxybutylene alcohol dithiophosphate and alkyl dithiocarbonate in a weight ratio of 3:1 is added to the phosphogypsum mixed slurry, and the addition amount of the composite flotation agent is 0.04% of the weight of the phosphogypsum mixed slurry, and column classification flotation is performed to obtain a phosphogypsum mixed slurry from which impurities are preliminarily removed;

[0035] (2) dehydrating the phosphogypsum mixed slurry obtained in step (1) by high-speed centrifugation at 20,000 r / min to obtain a hydrated phosphogypsum powder having a water content of less than 15%;

[0036] ⑶ The hydrated phosphogypsum powder obtained in step (2) is fed into an electromagnetic rotary furnace, and the first temperature control zone (preheating temperature control zone) is set to 100°C, the second temperature control zone (drying and desorption temperature control zone) is set to 150°C, the third temperature control zone (first de-crystallization temperature control zone) is set to 220°C, the fourth temperature control zone (second de-crystallization temperature control zone) is set to 230°C, the fifth temperature control zone (third de-crystallization temperature control zone) is set to 250°C, and the sixth temperature control zone (constant temperature maintenance and impurity removal zone) is set to 250°C, and preheating, drying, desorption and de-crystallization are carried out in sequence, and the total time is controlled to be 1h: wherein, the first temperature control zone is preheated for 10min; the second temperature control zone is dried for 20min; the third to sixth temperature control zones are de-crystallized and de-impurized for 8min, 6min, 6min10min, respectively; and the phosphogypsum powder with a temperature of less than 250°C is obtained;

[0037] (4) The phosphogypsum powder with a temperature below 250° C. obtained in step (3) is fed into a rotary cooling furnace and rapidly cooled to room temperature through water circulation; thereby obtaining phosphogypsum powder that can be used as a building material.

[0038] After testing, the phosphogypsum powder used as building materials obtained in step (4) has a whiteness of 89 according to the method specified in the national standard GB / T5950-2008 "Measurement method for whiteness of building materials and non-metallic mineral products"; a CaSO4 content of 95.13% according to the method specified in the national standard GB / T 5484-2009 "Chemical analysis method for gypsum"; and a flexural strength of 6.7 Mpa, a compressive strength of 58.1 Mpa, an initial setting time of 6.2 min, and a final setting time of 28.5 min according to the method specified in the national standard GB / T 17669.3-1999 "Determination of mechanical properties of building gypsum". The gypsum powder is a good building material.

[0039] Example 2

[0040] (1) preparing a phosphogypsum mixed slurry with 300 mesh phosphogypsum powder and water, wherein the water accounts for 70 wt % and the phosphogypsum powder accounts for 30 wt %, adding a composite flotation agent of polyoxybutylene alcohol dithiophosphate and alkyl dithiocarbonate in a weight ratio of 4:1 to the phosphogypsum mixed slurry, wherein the addition amount of the composite flotation agent is 0.05% of the weight of the phosphogypsum mixed slurry, and performing column classification flotation to obtain a phosphogypsum mixed slurry from which impurities are removed;

[0041] (2) dehydrating the phosphogypsum mixed slurry obtained in step (1) by high-speed centrifugation at 20,000 r / min to obtain a hydrated phosphogypsum powder having a water content of less than 15%;

[0042] (3) The hydrated phosphogypsum powder obtained in step (2) is fed into an electromagnetic rotary furnace, and the temperature is automatically controlled in stages, with the first temperature control zone set to 100° C., the second temperature control zone set to 150° C., the third temperature control zone set to 220° C., the fourth temperature control zone set to 280° C., the fifth temperature control zone set to 320° C., and the sixth temperature control zone set to 350° C., and preheating, drying, removing attached water, removing crystallization water, and burning off residual impurities not removed in the flotation process are performed in sequence, and the total time is controlled to be 1.2 h (72 minutes), wherein the first temperature control zone has a preheating time of 12 min; the second temperature control zone: the drying time is 24 min; the third to sixth temperature control zones are respectively for stepwise removal of crystallization water and impurity removal, and the time is 10 min, 7 min, 7 min, and 12 min, respectively; and the phosphogypsum powder with a temperature below 360° C. is obtained;

[0043] (4) the phosphogypsum powder obtained in step (3) at a temperature below 360° C. is fed into a rotary cooling furnace and rapidly cooled to room temperature through water circulation to obtain phosphogypsum powder, i.e. calcium sulfate powder; the room temperature refers to the indoor ambient temperature;

[0044] (5) The phosphogypsum powder obtained in step (4) is fed into an ultrafine roller mill for fine grinding to obtain a calcium sulfate powder product with an average particle size of 10 μm that can be used as a high-performance filler.

[0045] After testing, the calcium sulfate powder product obtained in step (5) was tested by Changsha Mineral Resources Supervision and Inspection Center (Hunan Geological Testing Institute) according to the method specified in national standard GB / T5950 "Whiteness Measurement Method for Building Materials and Non-metallic Mineral Products", with a whiteness of 92; tested according to the method specified in national standard GB / T 5484-2009 "Chemical Analysis Method for Gypsum", with a CaO content of 40.56%, a SO3 content of 57.90%, a total calcium sulfate content of 98.46%, and no crystal water; and had good compatibility with plastics, rubbers, and polyesters, and good biopolymerization with polylactic acid.

[0046] The test shows that the calcium sulfate powder produced in Example 2 of the present invention has good thermal stability and no phase change at 400°C. The application test commissioned by Changsha Frontier Plastic Technology Development Co., Ltd. shows that the use of the calcium sulfate powder obtained in Example 2 of the present invention as a filler in the production of LLDPE, LDPE, HDPE, PP and other products can improve the gloss, tensile strength, ductility, and opening of the product, improve the impact strength, and reduce deformation (see Table 1). It is confirmed that it has good compatibility with plastics, rubbers, and polyesters, and has good biopolymerization with polylactic acid; it is very suitable for use as a filler in the manufacture of plastics, rubbers, polyesters, and polylactic acid products.

[0047] The mechanical properties of the product produced by using the calcium sulfate powder produced in Example 2 of the present invention as a filler were tested: the impact resistance was tested using an Asrui free fall impact tester according to the method specified in the national standard GB / T2423.7-2018; the tensile strength, elongation at break, right-angle tear strength, and right-angle tear load of the film were tested using a Quanli KN series tensile tester according to the method specified in the national standard GB / T20671.7-2006; the optical properties of the film were tested: transmittance and haze were tested using an ASTM series haze tester according to the method specified in the national standard GB / T31370-2015.

[0048] The following are the relevant test data.

[0049] Table 1: Changsha Frontier Plastic Technology Development Co., Ltd. Application Example 2 Product Test Report Data

[0050]

[0051] The four fillers of calcium sulfate powder obtained in Example 2, commercial talcum powder, barium sulfate powder and calcium carbonate powder were mixed with the basic resin (LDPE 80% + LLDPE 20%) in a ratio of 15%:85% and then blown into film. The mechanical properties of the film are shown in Table 2; the optical properties are shown in Table 3. As can be seen from Table 2, the tensile strength of the film with the calcium sulfate powder filler obtained by the present invention is as high as 18.13MPa, which is 35.40% higher than that of the film with the talcum powder filler; 21.35% higher than that of the film with the expensive barium sulfate powder filler (see Table 5); and 67.72% higher than that of the film with the calcium carbonate powder filler. As can be seen from Table 3, the film with the calcium sulfate powder filler obtained by the present invention has the highest light transmittance, reaching 90.9%.

[0052] Table 2: Mechanical properties of several plastic films

[0053]

[0054] Table 3 Optical properties of several plastic films

[0055]

[0056] The three fillers of calcium sulfate powder obtained in Example 2, commercial talcum powder and calcium carbonate powder were mixed with polyethylene resin in a ratio of 15%:85%, and appropriate additives were added as usual. The mechanical properties of the polyethylene double-wall corrugated pipe are shown in Table 4. As can be seen from Table 4, the polyethylene double-wall corrugated pipe with the filler calcium sulfate powder obtained in Example 2 of the present invention has the best impact resistance, and none of them broke after 10 drop hammer impacts; the one with talcum powder broke 4 out of 10 drop hammer impacts.

[0057] Table 4 Physical and mechanical properties of polyethylene double-wall corrugated pipes with different fillers

[0058]

[0059] Table 5 Prices of several plastic film fillers

[0060] Filler Type Sales price (yuan / ton) Production Company Calcium sulfate powder 1600 Guizhou Kailin Group talcum powder 1550 Yantai Yongmei Chemical Barium sulfate powder 4250 Hunan Hechuang Chemical Calcium carbonate powder 750 Jiangxi Guangyuan Chemical

Claims

1. A method for purifying and whitening phosphogypsum, characterized in that: The following steps are involved: (1) preparing a mixed slurry of industrial solid waste phosphogypsum powder and water, and then adding a composite flotation agent to the phosphogypsum mixed slurry for flotation to obtain a phosphogypsum mixed slurry from which impurities have been preliminarily removed; the flotation is column classification flotation; (2) placing the phosphogypsum mixed slurry obtained in step (1) in a high-speed centrifugal dehydrator for centrifugal dehydration to obtain a hydrated phosphogypsum powder having a water content of less than 15%; (3) feeding the hydrated phosphogypsum powder obtained in step (2) into an electromagnetic rotary furnace, and sequentially performing preheating, drying, desorption of attached water, stepwise desorption of crystallization water, and calcination through staged temperature control, with the temperature gradually increasing, and sequentially removing attached water, crystallization water, and residual impurities not removed in the flotation process of step (1) in the hydrated phosphogypsum powder, to obtain phosphogypsum powder with a temperature of less than 360° C.; The segmented temperature control is as follows: the first temperature control zone, i.e. the preheating temperature control zone, is set at 80°C-100°C, the second temperature control zone, i.e. the drying and desorption temperature control zone, is set at 120°C-150°C, the third to fifth temperature control zones, i.e. the stepwise desorption temperature control zones, are set at 220°C-320°C, and the sixth temperature control zone, i.e. the desorption temperature control zone, is set at 300°C-360°C; the time control of each section is as follows: the first temperature control zone: preheating time 10min-15min; the second temperature control zone: drying time 20min-25min; the third to sixth temperature control zones, the stepwise desorption and desorption time and the desorption time of impurities by burning are 30min-40min in total, and the total time of preheating, drying and desorption, desorption and desorption, and desorption by burning are controlled at 0.9h-1.5h; (4) The phosphogypsum powder obtained in step (3) and having a temperature below 360° C. is fed into a rotary cooling furnace and rapidly cooled to room temperature through water circulation to obtain calcium sulfate powder.

2. The method for purifying and whitening phosphogypsum according to claim 1, characterized in that: The method further comprises the step (5): feeding the calcium sulfate powder obtained in the step (4) into an ultrafine grinding machine for fine grinding to obtain calcium sulfate powder with a mesh size of 1200-6000 which can be used as a high-performance filler.

3. The method for purifying and whitening phosphogypsum according to claim 2, characterized in that: In step (1), the particle size of the phosphogypsum powder is 200-350 mesh.

4. The method for purifying and whitening phosphogypsum according to claim 3, characterized in that: In step (1), the particle size of the phosphogypsum powder is 250-300 mesh.

5. The method for purifying and whitening phosphogypsum according to any one of claims 1 to 4, characterized in that: In step (1), in the phosphogypsum mixed slurry, the phosphogypsum powder accounts for 25-35wt%, and the water accounts for 65-75wt%.

6. The method for purifying and whitening phosphogypsum according to claim 5, characterized in that: In the phosphogypsum mixed slurry, the phosphogypsum powder accounts for 30% and the water accounts for 70wt%.

7. The method for purifying and whitening phosphogypsum according to any one of claims 1 to 4, characterized in that: In step (1), the composite flotation agent is prepared by mixing polyoxybutylene alcohol dithiophosphate and alkyl dithiocarbonate.

8. The method for purifying and whitening phosphogypsum according to claim 7, characterized in that: In the composite flotation agent, the weight ratio of the polyoxybutene alcohol dithiophosphate to the alkyl dithiocarbonate is 1-5:

1.

9. The method for purifying and whitening phosphogypsum according to claim 8, characterized in that: In the composite flotation agent, the weight ratio of the polyoxybutene alcohol dithiophosphate to the alkyl dithiocarbonate is 3-4:

1.

10. The method for purifying and whitening phosphogypsum according to any one of claims 1 to 4, characterized in that: In step (1), the addition amount of the composite flotation agent is 0.01-0.05% of the weight of the phosphogypsum mixed slurry.

11. The method for purifying and whitening phosphogypsum according to any one of claims 1 to 4, characterized in that: In step (2), the rotation speed of the high-speed centrifugal dehydrator is 8000-30000r / min.

12. The method for purifying and whitening phosphogypsum according to claim 11, characterized in that: In step (2), the rotation speed of the high-speed centrifugal dehydrator is 20000-25000r / min.

13. The method for purifying and whitening phosphogypsum according to any one of claims 1 to 4, characterized in that: In step (3), the total time for preheating, drying to remove attached water, removing crystal water, and burning to remove impurities is controlled to be 1h-1.2h.

Citation Information

Patent Citations

  • Method for producing PP (Polypropylene) material by taking ardealite as packing

    CN105330966A

  • Powdery ardealite filler and preparation thereof

    CN105331009A

  • Novel utilization method of phosphogypsum

    CN105524325A

  • Phosphogypsum treating agent, phosphogypsum treating method, preparation method of phosphogypsum filling material and phosphogypsum filling material

    CN111377632A

  • Comprehensive utilization method of phosphogypsum

    CN106145175A