Ceramic composite resin material and cable protective sheath

By using low-density polyethylene, linear low-density polyethylene and polyolefin resin in ceramic composite resin materials, combined with ceramic powder and flame retardant, the problem of insufficient mechanical properties of traditional ceramic polymer composite materials is solved, and the problem of insufficient mechanical properties of traditional ceramic polymer composite materials is achieved. UL94V0 flame retardant grade and good mechanical properties ensure the stability of the cable under high temperature fire conditions.

CN116120648BActive Publication Date: 2024-11-26HUANGPU INST OF MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211474586.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-11-26
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Traditional ceramic polymer composites have problems with insufficient mechanical properties in flame retardant grade UL94V0, which is difficult to meet the actual requirements.

Method used

Low-density polyethylene, linear low-density polyethylene and polyolefin resin are used as resin matrix, combined with ceramicized powder and flame retardant, and ceramicized composite resin materials are prepared through high-speed blending machines and pelletizing mechanisms to ensure that there is no heavy metals. The addition of halogen compounds and harmful substances can achieve good flame retardant effects and mechanical properties.

Benefits of technology

It achieves the improvement of the mechanical properties of ceramic composite resin materials while achieving the UL94V0 flame retardant level, ensuring the stability and integrity of the cable under high temperature and fire conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a ceramic composite resin material and a cable protective sleeve. The ceramic composite resin material comprises the following raw materials in percentage by mass: 45% to 70% of a resin matrix, 10% to 30% of a ceramic powder, 10% to 30% of a flame retardant, and 1% to 3% of an auxiliary agent, wherein the resin matrix comprises low-density polyethylene, linear low-density polyethylene, and polyolefin resin in a mass ratio of (50 to 80): (12 to 25): (2 to 5). The ceramic composite resin material is prepared by selecting low-density polyethylene, linear low-density polyethylene, and polyolefin resin as the resin matrix, and then coordinating the ceramic powder, the flame retardant, and the auxiliary agent. No harmful substances such as heavy metals, halogen compounds, and phthalates are added to the raw materials, and finally a good flame retardant effect is achieved. The flame retardant grade reaches UL94V0, and the material also has good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to a ceramic composite resin material and a cable protective sleeve. Background Art

[0002] Polymer materials have unique advantages in cable preparation, with good mechanical properties, light weight and good insulation, but they have certain defects in flame retardancy. Ceramic polymer composites have both the excellent properties of polymers at room temperature and the excellent properties of ceramics at high temperatures, and are widely used in fire prevention and heat protection. The emergence of ceramic polymers provides people with new countermeasures for dealing with sudden fire situations. The ceramic effect is mainly achieved by adding ceramic fillers. The ceramic filler system is mainly composed of ceramic fillers and flux. The ceramicization of polymer composites is to form a porous ceramic structure with good barrier properties and a certain degree of self-support on its surface when facing high temperature or fire, which can protect most materials from heat and open flames. For example, ceramic silicone rubber materials, ceramic composites of silicone rubber are the most popular materials in the cable industry, mainly because they have the ability to protect the internal core wire from thermal melting and maintain the stability of the cable at high temperatures, and even maintain the integrity of the line in a fire for up to 120 minutes or at high temperatures. During this period, all important public fire-fighting facilities, such as fire sprinklers, warning lights, alarm systems, etc., can work normally, thereby increasing the chances of evacuating people from the fire area.

[0003] Although traditional ceramic polymer composites can meet the flame retardant grade UL94V0 by not adding halides and other toxic and hazardous substances such as phthalates, there is still a problem that the mechanical properties cannot meet the actual requirements. Summary of the invention

[0004] Based on this, in order to improve the mechanical properties of the ceramic composite resin while ensuring that the flame retardant effect reaches the flame retardant grade UL94V0, it is necessary to provide a ceramic composite resin material and a cable protective cover.

[0005] The present invention provides a ceramic composite resin material, which comprises the following raw materials in terms of mass percentage:

[0006]

[0007] The resin matrix comprises low-density polyethylene, linear low-density polyethylene and polyolefin resin in a mass ratio of (50-80):(12-25):(2-5).

[0008] In one embodiment, the resin matrix satisfies one or more of the following characteristics:

[0009] (1) The melt index of the low-density polyethylene is 0.5 g / 10 min to 2.5 g / 10 min;

[0010] (2) The melt index of the linear low-density polyethylene is 1.5 g / 10 min to 3.0 g / 10 min;

[0011] (3) The melt index of the polyolefin resin is 1.0 g / 10 min to 10.0 g / 10 min.

[0012] In one embodiment, the ceramic powder is selected from one or more of mica powder, silicon powder, zinc borate powder, alumina trihydrate powder and zinc oxide powder.

[0013] In one embodiment, the ceramic powder includes mica powder, silicon powder, zinc borate powder, alumina trihydrate powder and zinc oxide powder in a mass ratio of (28-55):(18-25):(8-18):(8-25):(3-18).

[0014] In one embodiment, the flame retardant is selected from one or more of microcapsule-encapsulated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin.

[0015] In one embodiment, the flame retardant includes microcapsule-encapsulated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of (30-55):(18-28):(18-36):(4-15).

[0016] In one embodiment, the auxiliary agent includes an antioxidant, a coupling agent and a lubricant in a mass ratio of (0.1-1):(0.1-1):(0.1-2).

[0017] In one embodiment, the resin matrix further includes one or more of styrene-butadiene-styrene block copolymer and ethylene-vinyl acetate copolymer.

[0018] Furthermore, the present invention also provides a cable protective cover, comprising the above-mentioned ceramic composite resin material.

[0019] The above-mentioned ceramic composite resin material selects low-density polyethylene, linear low-density polyethylene and polyolefin resin as the resin matrix, and cooperates with ceramic powder, flame retardant and additives. There is no need to add heavy metals, halogen compounds, phthalates and other harmful substances to the raw materials. Finally, a good flame retardant effect is achieved. The flame retardant grade reaches UL94V0 and it also has good mechanical properties. DETAILED DESCRIPTION

[0020] The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or letters in different examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed.

[0021] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present invention, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0022] Unless otherwise indicated, all percentages, fractions and ratios are calculated based on the total mass of the composition of the present invention. Unless otherwise indicated, all masses of listed ingredients are given as active substances, so they do not include solvents or by-products that may be contained in commercially available materials. The term "mass percentage content" herein may be represented by the symbol "%".

[0023] As used herein, "includes," "comprising," "including," "containing," "having," or other variations are intended to encompass non-closed inclusions, and no distinction is made between these terms. The term "comprising" means that other steps and ingredients that do not affect the end result may be added. The term "comprising" also includes the terms "consisting of" and "consisting essentially of." The compositions and methods / processes of the present invention comprise, consist of, and consist essentially of the essential elements and limitations described herein, as well as any additional or optional ingredients, components, steps, or limitations described herein. As used herein, no distinction is made between the terms "efficacy," "performance," "effect," and "efficacy."

[0024] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0025] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0027] The present invention provides a ceramic composite resin material, which comprises the following raw materials in terms of mass percentage:

[0028]

[0029] The resin matrix includes low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) in a mass ratio of (50-80):(12-25):(2-5).

[0030] Furthermore, the ceramic composite resin material includes the following raw materials in terms of mass percentage:

[0031]

[0032] In a specific example, the ceramic composite resin material is composed of the following raw materials, by mass percentage: 50% of a resin matrix, 28% of a ceramic powder, 20% of a flame retardant, and 2% of an auxiliary agent.

[0033] In a specific example, the ceramic composite resin material is composed of the following raw materials, by mass percentage: 60% of a resin matrix, 25% of a ceramic powder, 13% of a flame retardant, and 2% of an auxiliary agent.

[0034] In a specific example, the ceramic composite resin material is composed of the following raw materials, by mass percentage: 55% of resin matrix, 15% of ceramic powder, 28% of flame retardant and 2% of auxiliary agent.

[0035] In a specific example, the ceramic composite resin material is composed of the following raw materials, by mass percentage: 65% of a resin matrix, 15% of a ceramic powder, 18% of a flame retardant, and 2% of an auxiliary agent.

[0036] In a specific example, the melt index of low-density polyethylene (LDPE) is 0.5 g / 10 min to 2.5 g / 10 min. It can be understood that the melt index of low-density polyethylene (LDPE) can be but is not limited to 0.5 g / 10 min, 1 g / 10 min, 1.5 g / 10 min, 2 g / 10 min or 2.5 g / 10 min. Preferably, the melt index of low-density polyethylene (LDPE) is 1.5 g / 10 min.

[0037] In a specific example, the melt index of linear low density polyethylene (LLDPE) is 1.5 g / 10 min to 3.0 g / 10 min. It can be understood that the melt index of linear low density polyethylene (LLDPE) can be but is not limited to 1.5 g / 10 min, 2 g / 10 min, 2.5 g / 10 min or 3 g / 10 min. Preferably, the melt index of linear low density polyethylene (LLDPE) is 2 g / 10 min.

[0038] In a specific example, the melt index of the polyolefin resin (POE) is 1.0 g / 10 min to 10.0 g / 10 min. It can be understood that the melt index of the polyolefin resin (POE) can be but is not limited to 1 g / 10 min, 2 g / 10 min, 3 g / 10 min, 4 g / 10 min, 5 g / 10 min, 6 g / 10 min, 7 g / 10 min, 8 g / 10 min, 9 g / 10 min or 10 g / 10 min.

[0039] Preferably, the resin matrix comprises low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) in a mass ratio of 50:25:5; or the resin matrix comprises low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) in a mass ratio of 75:12:2; or the resin matrix comprises low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) in a mass ratio of 70:15:5; or the resin matrix comprises low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) in a mass ratio of 80:15:5.

[0040] In a specific example, the ceramic powder is selected from one or more of mica powder, silicon powder, zinc borate, alumina trihydrate and zinc oxide.

[0041] In a specific example, the ceramic powder includes mica powder, silica powder, zinc borate powder, alumina trihydrate powder and zinc oxide powder in a mass ratio of (28-55):(18-25):(8-18):(8-25):(3-18). Preferably, it includes mica powder, silica powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of (30-50):(20-23):(10-17):(10-20):(5-15).

[0042] Preferably, the above-mentioned ceramic powder includes mica powder, silica powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 50:20:10:10:10; or the above-mentioned ceramic powder includes mica powder, silica powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 30:20:15:20:15; or the above-mentioned ceramic powder includes mica powder, silica powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 38:20:12:20:10; or the above-mentioned ceramic powder includes mica powder, silica powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 40:23:17:15:5.

[0043] Furthermore, the particle size D50 of the ceramic powder is 3 μm to 5 μm. It can be understood that the particle size D50 of the ceramic powder can be but is not limited to 3 μm, 4 μm or 5 μm. Preferably, the ceramic powder can pass through a 3000 mesh sieve.

[0044] In a specific example, the flame retardant is selected from one or more of microcapsule-encapsulated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methylphenyl silicone resin.

[0045] In a specific example, the flame retardant includes microcapsule-coated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of (30-55):(18-28):(18-36):(4-15), preferably microcapsule-coated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of (32-50):(20-28):(20-35):(5-13).

[0046] Preferably, the flame retardant includes microcapsule-coated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 50:25:20:5; or the flame retardant includes microcapsule-coated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 32:28:35:5; or the flame retardant includes microcapsule-coated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 42:20:25:13; or the flame retardant includes microcapsule-coated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 40:28:20:12.

[0047] In a specific example, the auxiliary agent is selected from one or more of an antioxidant, a coupling agent and a lubricant.

[0048] In a specific example, the additive includes an antioxidant, a coupling agent, and a lubricant in a mass ratio of (0.1-1):(0.1-1):(0.1-2).

[0049] Further, the coupling agent is a silane coupling agent, which may be, but is not limited to, one or more selected from vinyl triethoxy silane coupling agent, vinyl trimethoxy silane coupling agent and vinyl tri(β-methoxyethoxy) silane coupling agent.

[0050] Furthermore, the antioxidant may be, but is not limited to, one or more selected from the group consisting of antioxidant 1010 , antioxidant 2264 , antioxidant CA, and antioxidant 1076 .

[0051] It can be understood that the lubricant can be, but is not limited to, one or more selected from oxidized polyethylene wax, tristearate glyceryl, calcium stearate and zinc stearate.

[0052] Preferably, the auxiliary agent includes an antioxidant, a coupling agent and a lubricant in a mass ratio of 0.5:0.5:1.

[0053] In a specific example, the composite resin material further includes one or more of styrene-butadiene-styrene block copolymer (SBS) and ethylene-vinyl acetate copolymer (EVA).

[0054] Furthermore, the resin matrix composition is low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE), styrene-butadiene-styrene block copolymer (SBS) and ethylene-vinyl acetate copolymer (EVA) in a mass ratio of (50-80):(12-25):(2-5):(0-10):(0-10).

[0055] It can be understood that the resin matrix in the composite resin material is composed of low-density polyethylene, linear low-density polyethylene and polyolefin resin, or is composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE), styrene-butadiene-styrene block copolymer (SBS) and ethylene-vinyl acetate copolymer (EVA), or is composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE) and ethylene-vinyl acetate copolymer (EVA).

[0056] In a specific example, the styrene-butadiene-styrene block copolymer (SBS) is a linear styrene-butadiene-styrene block copolymer (SBS), and the average relative molecular weight of the styrene-butadiene-styrene block copolymer (SBS) is 80,000 to 120,000.

[0057] In a specific example, the mass percentage of vinyl acetate (VA) in ethylene-vinyl acetate copolymer (EVA) is 5% to 28%. It can be understood that the mass percentage of vinyl acetate (VA) can be but is not limited to 5%, 7%, 9%, 11%, 13%, 14%, 16%, 18%, 20%, 22%, 24%, 26% or 28%, preferably 14%.

[0058] Furthermore, the resin matrix composition includes low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE), styrene-butadiene-styrene block copolymer (SBS) and ethylene-vinyl acetate copolymer (EVA) in a mass ratio of 50:25:5:10:10.

[0059] Furthermore, the resin matrix composition includes low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE), styrene-butadiene-styrene block copolymer (SBS) and ethylene-vinyl acetate copolymer (EVA) in a mass ratio of 75:12:2:3:8.

[0060] Specifically, the resin matrix composition includes low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE) and ethylene-vinyl acetate copolymer (EVA) in a mass ratio of 70:15:5:10.

[0061] In a specific example, the resin matrix composition includes low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) in a mass ratio of 80:15:5.

[0062] The above-mentioned ceramic composite resin material selects low-density polyethylene, linear low-density polyethylene and polyolefin resin as the resin matrix, and cooperates with ceramic powder, flame retardant and additives. No heavy metals, halogen compounds, phthalates and other harmful substances are added to the raw materials. Finally, a good flame retardant effect is achieved. The flame retardant grade reaches UL94V0 and it also has good mechanical properties.

[0063] It can be understood that the preparation method of the ceramic composite resin material comprises the following steps:

[0064] (1) preparing the raw materials according to the mass ratio of the above raw materials, mixing them, putting them into a high-speed blender and mixing them evenly to obtain a mixed material;

[0065] (2) extruding and granulating the mixture through an internal mixer granulator to prepare the ceramic composite resin material;

[0066] Among them, the extrusion conditions are shown in the following table.

[0067]

[0068] Furthermore, the present invention also provides the use of the above composite resin material in preparing a cable protective sheath.

[0069] The following specific embodiments are provided to further illustrate the ceramic composite resin material and the cable protective sleeve of the present invention. The raw materials involved in the following specific embodiments, unless otherwise specified, can all be commercially available, wherein LDPE is purchased from Sinopec Model 951 or Shell Model 2426H, LLDPE is purchased from Sinopec Model 7042 or Shell Model 7042, POE is purchased from Dow Chemical Model 9100, SBS is purchased from LG Chemical Model LG501S, and EVA is purchased from Yangzi Petrochemical Model V5110J.

[0070] Example 1

[0071] This embodiment provides a ceramic composite resin, which includes, by mass percentage, 50% of a resin matrix, 28% of a ceramic powder, 20% of a flame retardant, and 2% of an additive.

[0072] The resin matrix is ​​composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE), styrene-butadiene-styrene block copolymer (SBS) and ethylene-vinyl acetate copolymer (EVA) in a mass ratio of 50:25:5:10:10.

[0073] The ceramic powder is composed of mica powder, silicon powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 50:20:10:10:10.

[0074] The flame retardant is composed of microcapsule-encapsulated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 50:25:20:5.

[0075] The auxiliary agent consists of antioxidant 1010, vinyl trimethoxy silane coupling agent and oxidized polyethylene wax lubricant in a mass ratio of 0.5:0.5:1.

[0076] The preparation method of the ceramic composite resin is as follows: prepare the raw materials according to the mass ratio, mix them, put them into a high-speed blender and mix them evenly to obtain a mixture; extrude and granulate the mixture through a mixing granulator under the conditions shown in the table below to prepare the ceramic composite resin material.

[0077]

[0078] Example 2

[0079] This embodiment provides a ceramic composite resin, which includes, by mass percentage, 60% of a resin matrix, 25% of a ceramic powder, 13% of a flame retardant, and 2% of an additive.

[0080] The resin matrix is ​​composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE), styrene-butadiene-styrene block copolymer (SBS) and ethylene-vinyl acetate copolymer (EVA) in a mass ratio of 75:12:2:3:8.

[0081] The ceramic powder is composed of mica powder, silicon powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 30:20:15:20:15.

[0082] The flame retardant is composed of microcapsule-coated red phosphorus, ethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 32:28:35:5.

[0083] The auxiliary agent consists of antioxidant 1010, vinyl trimethoxy silane coupling agent and oxidized polyethylene wax lubricant in a mass ratio of 0.5:0.5:1.

[0084] The preparation method of the ceramic composite resin is as follows: prepare the raw materials according to the mass ratio, mix them, put them into a high-speed blender and mix them evenly to obtain a mixture; extrude and granulate the mixture through a mixing granulator under the conditions shown in the table below to prepare the ceramic composite resin material.

[0085]

[0086] Example 3

[0087] This embodiment provides a ceramic composite resin, which includes, by mass percentage, 55% of a resin matrix, 15% of a ceramic powder, 28% of a flame retardant, and 2% of an additive.

[0088] The resin matrix is ​​composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyolefin resin (POE) and ethylene-vinyl acetate copolymer (EVA) in a mass ratio of 70:15:5:10.

[0089] The ceramic powder is composed of mica powder, silicon powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 38:20:12:20:10.

[0090] The flame retardant is composed of microcapsule-encapsulated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 42:20:25:13.

[0091] The auxiliary agent consists of antioxidant 1010, vinyl trimethoxy silane coupling agent and oxidized polyethylene wax lubricant in a mass ratio of 0.5:0.5:1.

[0092] The preparation method of the ceramic composite resin is as follows: prepare the raw materials according to the mass ratio, mix them, put them into a high-speed blender and mix them evenly to obtain a mixture; extrude and granulate the mixture through a mixing granulator under the conditions shown in the table below to prepare the ceramic composite resin material.

[0093]

[0094] Example 4

[0095] This embodiment provides a ceramic composite resin, which includes, by mass percentage, 65% of a resin matrix, 15% of a ceramic powder, 18% of a flame retardant, and 2% of an additive.

[0096] The resin matrix is ​​composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) in a mass ratio of 80:15:5.

[0097] The ceramic powder is composed of mica powder, silicon powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 40:23:17:15:5.

[0098] The flame retardant is composed of microcapsule-encapsulated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 40:28:20:12.

[0099] The auxiliary agent consists of antioxidant 1010, vinyl trimethoxy silane coupling agent and oxidized polyethylene wax lubricant in a mass ratio of 0.5:0.5:1.

[0100] The preparation method of the ceramic composite resin is as follows: prepare the raw materials according to the mass ratio, mix them, put them into a high-speed blender and mix them evenly to obtain a mixture; extrude and granulate the mixture through a mixing granulator under the conditions shown in the table below to prepare the ceramic composite resin material.

[0101]

[0102] Comparative Example 1

[0103] This comparative example provides a ceramic composite resin, which comprises, by mass percentage, 65% of a resin matrix, 15% of a ceramic powder, 18% of a flame retardant, and 2% of an additive.

[0104] The resin matrix is ​​composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) in a mass ratio of 5:15:10.

[0105] The ceramic powder is composed of mica powder, silicon powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 40:23:17:15:5.

[0106] The flame retardant is composed of microcapsule-encapsulated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 40:28:20:12.

[0107] The auxiliary agent consists of antioxidant 1010, vinyl trimethoxy silane coupling agent and oxidized polyethylene wax lubricant in a mass ratio of 0.5:0.5:1.

[0108] The preparation method of the ceramic composite resin is as follows: prepare the raw materials according to the mass ratio, mix them, put them into a high-speed blender and mix them evenly to obtain a mixture; extrude and granulate the mixture through a mixing granulator under the conditions shown in the table below to prepare the ceramic composite resin material.

[0109]

[0110] Comparative Example 2

[0111] This comparative example provides a ceramic composite resin, which comprises, by mass percentage, 65% of a resin matrix, 15% of a ceramic powder, 18% of a flame retardant, and 2% of an additive.

[0112] The resin matrix is ​​composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and styrene-butadiene-styrene block copolymer (SBS) in a mass ratio of 60:25:15.

[0113] The ceramic powder is composed of mica powder, silicon powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 50:20:10:10:10.

[0114] The flame retardant is composed of microcapsule-coated red phosphorus, ethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 32:28:35:5.

[0115] The auxiliary agent consists of antioxidant 1010, vinyl trimethoxy silane coupling agent and oxidized polyethylene wax lubricant in a mass ratio of 0.5:0.5:1.

[0116] The preparation method of the ceramic composite resin is as follows: prepare the raw materials according to the mass ratio, mix them, put them into a high-speed blender and mix them evenly to obtain a mixture; extrude and granulate the mixture through a mixing granulator under the conditions shown in the table below to prepare the ceramic composite resin material.

[0117]

[0118] Comparative Example 3

[0119] This comparative example provides a ceramic composite resin, which comprises, by mass percentage, 55% of a resin matrix, 15% of a ceramic powder, 28% of a flame retardant, and 2% of an additive.

[0120] The resin matrix is ​​composed of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and ethylene-vinyl acetate copolymer (EVA) in a mass ratio of 70:15:15.

[0121] The ceramic powder is composed of mica powder, silicon powder, zinc borate, alumina trihydrate and zinc oxide in a mass ratio of 50:20:10:10:10.

[0122] The flame retardant is composed of microcapsule-encapsulated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methyl phenyl silicone resin in a mass ratio of 42:20:25:13.

[0123] The auxiliary agent consists of antioxidant 1010, vinyl trimethoxy silane coupling agent and oxidized polyethylene wax lubricant in a mass ratio of 0.5:0.5:1.

[0124] The preparation method of the ceramic composite resin is as follows: prepare the raw materials according to the mass ratio, mix them, put them into a high-speed blender and mix them evenly to obtain a mixture; extrude and granulate the mixture through a mixing granulator under the conditions shown in the table below to prepare the ceramic composite resin material.

[0125]

[0126] The performance tests and results of the ceramic powders obtained in the above embodiments and comparative examples are shown in the following table:

[0127]

[0128] From the test results between the above-mentioned test comparative examples and the embodiments, it can be seen that the ratio between low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and polyolefin resin (POE) is not optimized in comparative example 1, and polyolefin resin (POE) is not added in comparative example 2, and the resin composition consists of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and styrene-butadiene-styrene block copolymer. Comparative example 3 does not add polyolefin resin (POE), and the resin composition consists of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE) and ethylene-vinyl acetate copolymer (EVA). It can be seen that although the mechanical properties of the ceramic powder obtained in the comparative example are improved to a certain extent, the flame retardancy is significantly reduced, indicating that not only the appropriate resin should be selected, but also the ratio of the resin should be within an appropriate range to meet the requirements of the present application for the mechanical properties of the ceramic powder and the requirements for its flame retardant properties.

[0129] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0130] The above-described embodiments only express several implementation methods of the present invention, which are convenient for understanding the technical solutions of the present invention in detail, but they cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided by the present invention are all within the protection scope of the claims attached to the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the contents of the attached claims, and the description can be used to interpret the contents of the claims.

Claims

1. A ceramic composite resin material, characterized in that: In terms of mass percentage, it includes the following raw materials: Resin matrix 45%~70%, Ceramic powder 10%~30%, Flame retardant 10%~30%, and Additives 1%~3%, The resin matrix is ​​composed of low-density polyethylene, linear low-density polyethylene, polyolefin resin, styrene-butadiene-styrene block copolymer and ethylene-vinyl acetate copolymer in a mass ratio of (50-80): (12-25): (2-5): (0-10): (0-10); The polyolefin resin is Dow Chemical Model 9100; The ceramic powder comprises mica powder, silicon powder, zinc borate powder, alumina trihydrate powder and zinc oxide powder in a mass ratio of (28-55): (18-25): (8-18): (8-25): (3-18); The flame retardant comprises microcapsule-coated red phosphorus, diethyl aluminum hypophosphite, magnesium hydroxide and methylphenyl silicone resin in a mass ratio of (30-55): (18-28): (18-36): (4-15); The auxiliary agent is composed of an antioxidant, a coupling agent and a lubricant in a mass ratio of (0.1~1): (0.1~1): (0.1~2).

2. The ceramic composite resin material according to claim 1, characterized in that: The melt index of the low-density polyethylene is 0.5 g / 10min to 2.5 g / 10min.

3. The ceramic composite resin material according to claim 1, characterized in that: The melt index of the linear low-density polyethylene is 1.5 g / 10min to 3.0 g / 10min.

4. The ceramic composite resin material according to claim 1, characterized in that: The melt index of the polyolefin resin is 1.0 g / 10min to 10.0 g / 10min.

5. The ceramic composite resin material according to claim 1, characterized in that: The D50 particle size of the ceramic powder is 3 μm to 5 μm.

6. The ceramic composite resin material according to claim 1, characterized in that: The antioxidant includes one or more of antioxidant 1010 , antioxidant 2264 , antioxidant CA and antioxidant 1076 .

7. The ceramic composite resin material according to claim 1, characterized in that: The coupling agent is a silane coupling agent.

8. The ceramic composite resin material according to claim 1, characterized in that: The lubricant is selected from one or more of oxidized polyethylene wax, tristearate glyceryl, calcium stearate and zinc stearate.

9. A cable protective cover, characterized in that: The ceramic composite resin material comprises the ceramic composite resin material according to any one of claims 1 to 8.