A high-strength steel plate with excellent cold bending performance and yield strength of 690MPa and a manufacturing method thereof

Through the design of low C and low Si chemical composition and Nb-V-Ti composite, combined with TMCP process and low temperature tempering, ferrite matrix and nano-scale precipitates are formed, which solves the problems of high cost and poor cold bending performance in the production of high-strength steel plates. , realizes efficient and low-cost high-strength steel plate production, with excellent cold bending and welding performance.

CN116121643BActive Publication Date: 2024-11-29JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211663142.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-11-29
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

In the existing high-strength steel plate production technology, in order to obtain high strength, precious metal alloying is often used, resulting in high costs, long production processes, poor cold bending performance and poor welding performance, making it difficult to achieve low cost, short process and excellent cold bending performance. production method.

Method used

Using low C and low Si chemical composition design, the precious metals such as Cr/Ni/Mo/Cu are eliminated, and Nb-V-Ti composite is adopted. Through TMCP process and low temperature tempering, a fine ferrite matrix structure and nanoscale TiC and NbC are formed. , significantly improve the strength and toughness of the steel plate and optimize cold bending performance.

Benefits of technology

It has achieved low-cost and efficient production of high-strength steel plates with excellent cold bending performance and yield strength of 690MPa, with excellent welding performance and low-temperature impact performance. The substrate structure of the steel plate is fine ferrite, which significantly improves the cold bending molding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004014768470000061
    Figure BDA0004014768470000061
  • Figure BDA0004014768470000062
    Figure BDA0004014768470000062
  • Figure BDA0004014768470000071
    Figure BDA0004014768470000071
Patent Text Reader

Abstract

The invention relates to a high-strength steel plate with excellent cold bending performance and a yield strength of 690MPa and a manufacturing method thereof. The steel plate comprises the following components by weight percentage: C: 0.04-0.08%, Si: <0.10%, Mn: 1.80-2.00%, Nb: 0.050%-0.080%, V: ≤0.020%, Ti: 0.11%-0.15%, Al: 0.03-0.06%, Ni: <0.10%, Cu: <0.10%, Cr: <0.010%, Mo: <0.010%, B: <0.001%, Ca: 0.001-0.005%, P: ≤0.012%, S: ≤0.002%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, and the remainder is Fe and unavoidable impurity elements; and the carbon equivalent CEV is ≤0.45%. The microstructure is composed of nano-sized TiC and NbC particles dispersed on a fine ferrite matrix, with a grain size of ≥7. Different from the martensite or bainite structure of traditional high-strength steel with a yield strength of 690MPa, the ferrite matrix is ​​relatively soft, which will greatly improve the cold bending performance of the steel plate, d=2a, and there is no crack in 90° cold bending.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron-based alloys, and in particular relates to a high-strength steel plate with good cold bending performance and a manufacturing method thereof. Background Art

[0002] With the rapid development of domestic and foreign steel structure industry, building bridges, engineering machinery, mining machinery and other industries, the market demand for 690MPa grade high-strength steel plates is increasing. Since high-strength steel plates often need to be processed into various shapes during use to meet the needs of engineering machinery equipment assembly, the cold bending performance of steel plates is crucial for the application of high-strength steel plates.

[0003] Traditional high-strength steel plates with a yield strength of 690MPa are generally produced by quenching + high-temperature tempering, which can improve strength while also satisfying toughness. However, in order to obtain high strength, this production method often uses precious metal alloys such as Cr, Ni, and Mo, which is costly and has a long production process. At the same time, it also leads to high carbon equivalent, poor welding performance, and decreased cold bending performance. How to use a short process and low cost method to produce easy-to-weld high-strength steel plates with excellent cold bending performance has gradually become one of the important development directions of major steel companies.

[0004] The patent document of Chinese patent publication number CN104988429A discloses a structural steel plate for bridges with a yield strength of 690MPa. The invention is produced by the traditional quenching + tempering process, and the carbon content is relatively low (C: 0.04-0.08%). In order to improve the strength and toughness, the invention adds precious metals such as Cr / Mo / Ni / Cu, which is costly and not conducive to promotion.

[0005] The patent document of Chinese Patent Publication No. CN101418418B discloses a low crack sensitivity steel plate with a yield strength of 690MPa and a method for manufacturing the same. The invention adopts a low-carbon bainite design (C: 0.03-0.06%) with good crack resistance; the TMCP process is used in the process. In order to increase the hardenability, the invented steel plate adds an appropriate amount of Cr, Mo, and B alloys, and at the same time adds a higher V content (V: 0.04-0.12%). The invention has a short production process, but the addition of Cr / Mo / V / B alloys leads to higher costs and reduced cold bending performance.

[0006] The Chinese patent publication number CN104278216A discloses that a structural steel plate for engineering machinery with a yield strength of 690 MPa has been developed by combining online quenching technology with a medium carbon composition design (C: 0.10-0.20%). The steel plate also contains hardenability elements such as Cr, Ni, Mo, and B.

[0007] In summary, the existing production technologies for high-strength steel plates with a yield strength of 690MPa mainly include quenching + tempering or online TMCP; the composition design mostly adopts Cr-Mo-B alloying to obtain a martensite or bainite structure with higher strength. However, martensite or bainite has high strength and low toughness, and the steel plate can generally only meet the cold bending requirements of d≥3a (d is the cold bending radius, a is the thickness of the bent steel plate). Summary of the invention

[0008] The object of the present invention is to provide a quenched and tempered high-strength steel plate with excellent cold bending performance and a yield strength greater than or equal to 690 MPa and a production method thereof.

[0009] To achieve the above object, the technical solution adopted by the present invention is: a quenched and tempered high-strength steel plate with excellent cold bending performance and a yield strength greater than or equal to 690MPa, the chemical composition of the steel plate is C: 0.04-0.08%, Si: <0.10%, Mn: 1.80-2.00%, Nb: 0.050%-0.080%, V: ≤0.020%, Ti: 0.11%-0.15%, Al: 0.03- 0.06%, Ni: <0.10%, Cu: <0.10%, Cr: <0.010%, Mo: <0.010%, B: <0.001%, Ca: 0.001~0.005%, P: ≤0.012%, S: ≤0.002%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, the balance is Fe and unavoidable impurity elements; Carbon equivalent CEV: ≤0.45%.

[0010] The thickness of the high-strength steel plate with excellent cold bending performance and yield strength of 690 MPa based on the above chemical composition is ≤12 mm.

[0011] The selection and content of steel components in the present invention are limited according to the following:

[0012] C: Carbon as a solid solution element can significantly improve the strength of the steel plate, but it has an adverse effect on the plasticity, toughness, cold bending performance and welding performance of the steel plate. Based on the requirements of steel plate strength and toughness matching and cold bending performance, the carbon content in the present invention is controlled to be 0.04-0.08%.

[0013] Si: Si enters ferrite to play a role in solid solution strengthening, but when the Si content is too high, oxidation spots are easily formed on the surface of the steel plate during rolling, the surface quality is reduced, and local stress concentration occurs during cold bending, affecting the cold bending performance of the steel plate. The Si content of the present invention is less than 0.10%, the surface quality of the steel plate is excellent, and it is conducive to improving the cold bending performance.

[0014] Mn: reduces the critical transformation temperature Ar3, improves the hardenability of the steel, plays a role of solid solution strengthening in the steel, and significantly improves the strength of the steel. The present invention stipulates that the amount of manganese added is within the range of 1.80-2.00%.

[0015] Nb: can produce significant grain refinement, precipitation strengthening and precipitation strengthening effects. Nb dissolved in austenite can improve hardenability, and the carbide precipitation phase of Nb has the effect of refining grains and improving matrix strength. In addition, the addition of relatively high Nb can increase the non-recrystallization temperature Tnr of steel plate rolling, so that finishing rolling can be carried out in a higher temperature range. In the present invention, the Nb content is controlled to be 0.050-0.080%. The main purposes are (1) to increase the finishing temperature so that the steel plate can be deformed at high temperature without recrystallization, fully refine the grains, and at the same time be beneficial to the surface quality of the steel plate and the cold bending forming performance of the steel plate; (2) the addition of relatively high Nb can precipitate a large amount of nano-NbC in the subsequent rolling and tempering process, significantly improving the strength of the steel plate.

[0016] Ti: An important alloying element of the present invention, a strong carbonitride-forming element, has the effect of refining grains during high-temperature rolling, improving the toughness and low-temperature toughness of steel; the nano-TiC precipitated during the low-temperature process can greatly improve the strength of the steel plate. The present invention eliminates the Cr-Mo-B alloying and mainly utilizes the low-temperature precipitation of nano-TiC to ensure that the yield strength of the steel plate is higher than 690MPa. However, when the Ti content is too high, especially when it is greater than 0.20%, it will lead to a decrease in the continuous casting quality, the formation of cracks, and the deterioration of the toughness of the steel plate. Therefore, the present invention controls the Ti content to 0.11% to 0.15%.

[0017] V: grain refining element; it can play a certain precipitation strengthening role during low temperature tempering. When the V content is too high, the toughness and welding performance of the steel plate will deteriorate. Therefore, the V content of the present invention is controlled to be ≤0.020%.

[0018] Al: deoxidizing and grain refining element. In the present invention, Al also plays the role of fixing N and preserving Ti, avoiding the formation of a large amount of TiN and reducing the strength and cold bending performance of the steel plate. The present invention stipulates that the Al content is 0.03-0.06%.

[0019] Cr: It is an element that improves the hardenability of steel, can inhibit the formation of polygonal ferrite and pearlite, promote the transformation of low-temperature microstructures bainite or martensite, and improve the strength of steel. However, too high a Cr content will affect the toughness of the steel and reduce the welding performance of the steel plate. The present invention adopts a ferrite matrix design to greatly improve the cold bending performance of the steel plate, so the addition of chromium is eliminated and the content is controlled to be less than 0.010%.

[0020] Mo: It is an element that improves the hardenability of steel and is beneficial to the formation of bainite or martensite during cooling. Adding a certain amount of Mo to the steel will increase the strength of the steel plate without affecting the low-temperature impact performance of the steel plate. Mo can increase the tempering resistance of the steel plate, so that the strength of the steel plate does not decrease at a higher temperature, but the cost of Mo is very high. In order to obtain a fine ferrite matrix structure, the present invention cancels the addition of molybdenum and controls the content to <0.010% in consideration of economic efficiency.

[0021] Ca: inclusion modifying element, which can react with long strips of MnS to generate spherical CaS, change the anisotropy of the steel plate, and can also modify the Al2O3 inclusions produced by Al deoxidation into spherical low-melting-point inclusions, promote the floating removal of inclusions, and improve the toughness and cold bending performance of the steel plate.

[0022] P: harmful element in steel, easy to segregate, adversely affecting the plasticity and toughness of the material. High P content increases the brittleness of the steel plate and easily causes cold bending cracking of the steel plate. The present invention stipulates that P: ≤ 0.012%

[0023] S: harmful element in steel, easy to segregate. Mn element easily forms MnS segregation inclusions, leading to delamination and cracking of steel plate, significantly reducing the cold bending performance of steel plate. Since the present invention adopts high Mn design, the S content must be controlled at a low level, and S is specified to be ≤0.002%.

[0024] O, H: harmful gas elements, high content, many inclusions, reduce the plastic toughness of the steel plate, and high risk of cracking of the steel plate. The present invention strictly controls the O content to be no higher than 0.002%; the H content to be no higher than 0.0002%.

[0025] N: harmful gas. The present invention uses nano-TiC to increase the strength of the steel plate. A high N content will form TiN inclusions with sharp corners, affecting the cold bending performance of the steel plate. Therefore, the present invention strictly controls the N content and stipulates that it is not higher than 0.004%;

[0026] CEV: The present invention adopts the carbon equivalent formula CEV = C + Mn / 6 + (Cr + Mo + V) / 5 + (Ni + Cu) / 15; carbon equivalent has a great influence on the strength and weldability of steel. High CEV has high strength, but reduced weldability; the present invention controls CEV ≤ 0.45.

[0027] The present invention further provides a method for preparing the above steel plate, which involves molten steel smelting, continuous casting, hot rolling, cooling and tempering, and the specific process is as follows:

[0028] Smelting and continuous casting process: Pre-treatment of molten iron, smelting in electric furnace or converter, then refining (sent to LF refining furnace), and vacuum degassing (VD or RH). After degassing, trace Ca treatment is carried out on the molten steel, that is, Ca wire is added to the molten steel. Continuous casting adopts low superheat pouring, argon protection pouring throughout the process and dynamic light pressure control, superheat is controlled at 5-20℃, center segregation of ingot is not higher than C1.0 level, and center porosity is not higher than 1.0 level.

[0029] Heating: It is preferred to place the ingot into a walking beam heating furnace. In order to reduce the impact of iron oxide on the surface quality of the steel plate and refine the grains, a lower heating temperature is used. The heating temperature of the ingot is controlled at 1100-1180°C and the heating time is 8-14min / cm.

[0030] Steel rolling: high-pressure water descaling is carried out before rolling the ingot, and the descaling pressure is controlled to be above 21MPa. The rough rolling temperature is ≥1000℃. High-pressure descaling is carried out in the odd-numbered passes and the last pass of rough rolling to fully remove the primary and secondary iron oxide scales. The temperature of the finishing rolling is controlled at ≥930℃. High-pressure water descaling is used in the finishing rolling, and the total number of descaling passes shall not be less than 3 passes. The final rolling temperature is controlled at a relatively low 780-840℃, so that the grains are fully deformed and refined, and the strength, toughness and cold bending performance of the steel plate are improved.

[0031] Post-rolling cooling: After rolling, the steel plate is cooled at an accelerated rate of ≥15°C / s, and the final cooling temperature is controlled at 420-520°C.

[0032] Tempering process: To ensure the precipitation of a large amount of nano-TiC, the steel plate needs to be tempered at a lower temperature. The tempering temperature is 450-550℃. After the furnace temperature reaches the temperature, the insulation time is 30-90min. To ensure the uniformity of the steel plate, the temperature control accuracy is ±10℃.

[0033] Compared with the prior art, the present invention has the following advantages:

[0034] The present invention adopts low C and low Si chemical composition design, eliminates the addition of precious metals such as Cr / Ni / Mo / Cu, and adopts economical Nb-V-Ti composite, which greatly reduces the alloy cost. The steel plate carbon equivalent CEV≤0.45 has excellent welding performance.

[0035] In terms of technology, the present invention adopts the TMCP short process to replace the traditional quenching process, which saves costs, releases production capacity, and reduces carbon emissions. The present invention performs tempering at a relatively low temperature to disperse and precipitate a large amount of nano-level TiC and NbC, significantly increasing the strength and plastic toughness of the steel plate.

[0036] The matrix structure of the steel plate of the present invention is fine ferrite with a grain size of ≥ grade 7. Different from the martensite or bainite structure of the conventional high-strength steel with a yield strength of 690 MPa, the ferrite matrix is ​​relatively soft, which will greatly improve the cold bending performance of the steel plate.

[0037] The steel plate has yield strength Rp0.2≥690MPa, tensile strength Rm≥770MPa, elongation A≥14%; -40℃ low temperature impact Akv≥100J. The steel plate has excellent cold bending performance, d=2a, and no cracks in 90° cold bending.

[0038] Obviously, the above-mentioned steel plate production method can also be extended and applied to other high-strength steel plates, such as high-strength offshore shipbuilding steel, high-rise building steel, bridge steel, engineering machinery steel, pressure vessel steel, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a SEM electron microscope scanning image (1000×) of the typical structure of the test steel in Example 1 of the present invention.

[0040] Figure 2 This is a SEM electron microscope scanning image (30000×) of typical nano-scale precipitates of the test steel of Example 1 of the present invention.

[0041] Figure 3 This is the energy spectrum analysis of nano-scale precipitates in the test steel of Example 2 of the present invention.

[0042] Figure 4 This is a cold bending photo of Example 2 of the present invention. DETAILED DESCRIPTION

[0043] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0044] The production process of high-strength steel with excellent cold bending performance in this application is: converter steelmaking->LF refining->VD or RH vacuum degassing->Ca treatment->continuous casting->heating->rolling->cooling->tempering.

[0045] The production method of the high-strength steel plate with a yield strength of 690 MPa of Example 1-2 specifically comprises the following steps:

[0046] (1) Steelmaking and continuous casting: 150-ton converter is used for smelting, then sent to LF furnace for refining and RH vacuum degassing treatment, and Ca treatment is performed by breaking the air. Molten steel is cast into 150 mm thick continuous casting billets. The casting temperature is controlled at 5-20 °C above the liquidus. Dynamic soft reduction is implemented during the casting process. The center segregation is not higher than C1.0 level, and the center porosity is not higher than 1.0 level. The final composition control of molten steel is shown in Table 1.

[0047] (2) Rolling and cooling: The continuous casting billet obtained in step (1) is placed in a walking beam heating furnace and heated to 1100-1180°C for 8-14 min / cm2 to fully dissolve the alloying elements in the steel to ensure the uniformity of the composition and performance of the final product. After the billet is removed from the furnace, it is descaled by high-pressure water and then subjected to two-stage controlled rolling of rough rolling + finishing rolling. The rolling temperature in the rough rolling recrystallization zone is controlled at 1000-1100°C; the finishing rolling start temperature is controlled at ≥930°C, and the final rolling temperature is controlled at 780-840°C to ensure that the steel plate finally obtains fine original austenite grains and improves the strength, toughness and cold bending performance of the steel plate. After rolling, the steel plate is accelerated cooled at a cooling rate of ≥15°C / s, and the final cooling temperature is controlled at 420-520°C. The relevant process parameters are shown in Table 2.

[0048] (3) Tempering: The tempering temperature of the steel plate is 450-550℃. After the furnace temperature reaches the temperature, the insulation time is 30-90 minutes.

[0049] The specific composition and process parameters are shown in Tables 1 to 3. The corresponding properties of each example sample are shown in Table 4.

[0050] Figure 1 The microstructure photograph of the test steel of Example 1 is given. The matrix structure of the steel plate is a fine ferrite structure, and the grain size of the structure is ≥ 7 levels, which ensures that the steel plate has excellent cold bending performance.

[0051] Figure 2 The SEM image of typical nano-scale precipitates of the test steel in Example 1 is given. Figure 3 This is the energy spectrum analysis of nano-scale precipitates in the test steel of Example 2. It can be seen that a large amount of nano-scale TiC and NbC are dispersed on the ferrite matrix of the steel plate, ensuring that the steel plate has excellent plasticity and toughness while also having ultra-high strength.

[0052] Figure 4 This is a cold bending picture of the test steel of Example 2. The cold bending radius d=2a, 90° without cracks, showing excellent cold bending forming performance.

[0053] The present invention adopts a high-cleanliness steelmaking continuous casting process, controlled rolling, controlled cooling and tempering process, and controls from the perspectives of chemical composition design, parent material structure, rolling deformation, tempering temperature and time, so as to ensure that the steel plate has high strength, high toughness and excellent cold bending performance. It can be widely used in the manufacture of large-scale engineering machinery equipment or steel structures such as high-rise buildings, bridges, and offshore platforms that have strict requirements on formability and weldability.

[0054] Table 1 Chemical composition of the super-strong steel plate of the embodiment (wt%)

[0055]

[0056] Table 2 Rolling process control

[0057]

[0058] Table 3 Heat treatment process control

[0059]

[0060] Table 4 Tensile, impact and bending properties of the embodiments of the present invention

[0061]

Claims

1. A high-strength steel plate with excellent cold bending performance and yield strength of 690MPa, characterized in that: The steel plate comprises the following components by weight percentage: C: 0.04-0.08%, Si: <0.10%, Mn: 1.80-2.00%, Nb: 0.050%-0.080%, V: 0.01-0.020%, Ti: 0.11%-0.15%, Al: 0.03-0.06%, Ni: <0.10%, Cu: <0.10%, Cr: <0.010%, Mo: <0.010%, B: <0.001%, Ca: 0.001-0.005%, P: ≤0.012%, S: ≤0.002%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, and the balance is Fe and inevitable impurity elements; carbon equivalent CEV≤0.45%; the microstructure of the steel plate is a dispersed distribution of nano-sized TiC and NbC particles on a fine ferrite matrix, with a grain size of ≥7; The production method of the steel plate includes molten steel smelting, continuous casting, hot rolling, cooling and tempering, wherein: (1) Molten steel smelting Converter smelting, refining outside the furnace and vacuum degassing are adopted in sequence, and Ca treatment is carried out after vacuum degassing. The chemical composition weight percentage of the molten steel is: C: 0.04-0.08%, Si: <0.10%, Mn: 1.80-2.00%, Nb: 0.050%-0.080%, V: ≤0.020%, Ti: 0.11%-0.15%, Al: 0.03-0.06%, Ni: <0.10%, Cu: <0.10%, Cr: <0.010%, Mo: <0.010%, B: <0.001%, Ca: 0.001-0.005%, P: ≤0.012%, S: ≤0.002%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, and the balance is Fe and inevitable impurity elements; Carbon equivalent CEV: ≤0.45%; Molten steel is cast into ingots by continuous casting process; (2) Heating rolling Heat the ingot to 1100℃-1180℃, the heating time is 8min / cm-14min / cm*ingot thickness cm, descale the ingot after it comes out of the furnace, control the rough rolling temperature ≥1000℃, descale the odd passes and the last pass, control the start temperature of the finishing rolling ≥930℃, descale the ingot at the start of the finishing rolling, the total descaling passes of the finishing rolling are not less than 3 passes, and the final rolling temperature is controlled at 780℃-840℃; (3) Cooling After rolling, the steel plate is cooled at an accelerated rate of ≥15°C / s, and the final cooling temperature is controlled at 420°C-520°C; (4) Tempering: The tempering temperature of the steel plate is 450℃-550℃. After the furnace temperature reaches the temperature, the insulation time is 30min-90min.

2. The high-strength steel plate with excellent cold bending performance and yield strength of 690 MPa according to claim 1, characterized in that: The production thickness of the steel plate is ≤12mm.

3. The high-strength steel plate with excellent cold bending performance and yield strength of 690 MPa according to claim 1, characterized in that: The yield strength of the steel plate is ≥690MPa, the tensile strength is ≥770MPa, and the elongation is ≥14%; the Charpy impact energy at -40℃ is ≥100J; d=2a, and there is no crack in 90° cold bending.

4. The high-strength steel plate with excellent cold bending performance and yield strength of 690 MPa according to claim 1, characterized in that: Argon protection is used throughout the continuous casting process to prevent the ingot from contacting the air. Dynamic light pressure is applied to the ingot during the continuous casting process, and the superheat of the molten steel is controlled at 5-20°C. The center segregation of the obtained ingot is not higher than C1.0 level, and the center porosity is not higher than 1.0 level.

5. The high-strength steel plate with excellent cold bending performance and yield strength of 690 MPa according to claim 1, characterized in that: The descaling in the method is performed by using high-pressure water of more than 21 MPa.

6. The high-strength steel plate with excellent cold bending performance and yield strength of 690 MPa according to claim 1, characterized in that: In step (1), the thickness of the ingot is greater than 150 mm.

Citation Information

Patent Citations

  • Low welding crack sensitivity steel plate with yield strength of 690MPa grade and method for producing the same

    CN101418418B

  • Steel plate with thickness of larger than 60mm and yield strength of 690MPa and preparation method of steel plate

    CN104278216A

  • Structure steel plate for bridge with yield strength being 690MPa and production method thereof

    CN104988429A

  • An economical high-strength steel plate with a yield strength of 690 MPa and its manufacturing method

    CN102260823A

  • High-strength steel plate with yield strength at 690MPa level and manufacture method thereof

    CN102888565A