A chemical crosslinking method suitable for preparing boron nitride fibers by organic precursor method
Through the chemical cross-linking method of alternating ammonia and non-ammonia atmospheres, the problems of low cross-linking efficiency, low ceramic yield and high cost in the preparation of boron nitride fibers in the existing technology have been solved, and the efficient preparation of boron nitride has been achieved. The dense morphology and excellent mechanical properties of the fiber.
Patent Information
- Application Number
- CN202310067632.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-16
AI Technical Summary
It is difficult to efficiently prepare boron nitride fibers with existing technology, especially the problem of maintaining high mechanical properties and dense morphology of boron nitride fibers while ensuring high cross-linking efficiency, high ceramic yield and low cost.
Boron nitride fibers are prepared by alternating between ammonia atmosphere and non-ammonia atmosphere or low-concentration ammonia atmosphere, cross-linking and non-melting treatment of boron nitride precursor fibers, followed by heat treatment to achieve inorganicization and ceramicization.
The ceramic yield and mechanical properties of boron nitride fiber are improved. The tensile strength of the fiber can reach 1.3GPa, the elastic modulus can reach 120GPa, and the fiber produced has a dense morphology, no hollows, and low cost.
Smart Images

Figure BDA0004063285120000031 
Figure BDA0004063285120000081 
Figure HDA0004063285130000011
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic fiber preparation of boron nitride fibers by a precursor conversion method, and in particular to a chemical crosslinking method suitable for preparing boron nitride fibers by an organic precursor method. Background Art
[0002] Boron nitride ceramics are a kind of artificial synthetic ceramics, which are nitride ceramics with a covalent bond structure. They have the characteristics of corrosion resistance, excellent high-temperature dielectric properties, low thermal expansion coefficient, thermal shock resistance, high thermal conductivity, excellent high-temperature dielectric properties and high-temperature mechanical properties. They can be used in oxidizing atmospheres at 900°C and inert atmospheres above 2000°C. They are a functional ceramic material.
[0003] At present, there are three main methods for preparing boron nitride ceramic products, namely high-temperature hot pressing, chemical vapor deposition and precursor conversion. High-temperature hot pressing is a traditional method for preparing boron nitride products. First, boron nitride powder must be prepared. Industrially, boron nitride powder is usually prepared by boron oxide and urea at high temperature, and then the boron nitride powder is sintered under high temperature and pressure to prepare boron nitride ceramic products. The chemical vapor deposition method for preparing boron nitride ceramics is to use boron-containing gas phase compounds and nitrogen-containing gas phase substances or gas phase compounds containing two elements of boron and nitrogen, and pyrolyze them at high temperature to form boron nitride materials. High-temperature hot pressing is a traditional process with mature technology, but it can only prepare block ceramic products with simple structure; chemical vapor deposition has low efficiency and high energy consumption, and is usually only suitable for preparing cost-effective thin film products, coatings, etc. The above two methods have their own advantages and disadvantages, but neither can prepare boron nitride ceramic fibers. In the 1960s, the route of preparing non-oxide ceramics by precursor conversion method was proposed. It uses suitable processable polymers to prepare products of specific shapes (such as fibers, films, etc.) by conventional methods, and then converts them into ceramic products of the desired form through infusible treatment, high-temperature pyrolysis, inorganicization and ceramicization. Since the 1980s, the preparation of boron nitride fibers by precursor conversion method has been one of the research hotspots in various countries. Kimura research team in Japan, Paine research team and Sneddon research team in the United States, Miele research team in France, etc. have all used polyborazane precursors and precursor conversion method to prepare boron nitride fibers.
[0004] The infusibility treatment of polyborazine precursor fiber or film usually adopts oxygen crosslinking or ammonia crosslinking. Oxygen crosslinking inevitably introduces a large amount of oxygen elements into the product, so that the final product boron nitride contains a large amount of oxygen, usually in the form of B2O3, which makes the boron nitride fiber easy to deliquesce; ammonia crosslinking is adopted, and no impurity elements are introduced during the crosslinking process, which can well solve the problem of impurities introduced by oxygen crosslinking. However, in order to ensure the spinnability of polyborazine, the polymerization degree of polyborazine is low and the molecular weight is small. While crosslinking under the action of ammonia, it is also easy to ammonolyze to form small molecular ammonolyze products, which volatilize during the heat treatment process, reduce the ceramic yield, affect the densification of the final product, and seriously hinder the formation of high-strength boron nitride fiber. The prior art discloses a method for preparing boron nitride fiber by crosslinking polyborazine with electron beam irradiation, which can reduce the problem of reduced ceramic yield caused by ammonolysis, but the electron beam irradiation equipment is complex, the production efficiency is low, the cost is high, and it is not conducive to large-scale promotion.
[0005] In summary, the invention provides a chemical crosslinking method for precursor boron nitride fibers with high crosslinking efficiency, high ceramic yield and low cost, which is of great significance to the field of precursor method for preparing boron nitride fibers. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a chemical crosslinking method suitable for preparing boron nitride fibers by the organic precursor method. The boron nitride precursor fibers are crosslinked and infusible treated in different atmospheres, and then inorganicized and ceramicized to obtain the boron nitride fibers. The method of the present invention has low preparation cost, high crosslinking efficiency, high ceramic yield, and the prepared boron nitride fibers have good morphology and mechanical properties.
[0007] The present invention adopts the following technical solutions:
[0008] A chemical crosslinking method for preparing boron nitride fibers by an organic precursor method comprises the following steps: subjecting the boron nitride precursor fibers to an alternating treatment in an ammonia atmosphere and a non-ammonia atmosphere or a low-concentration ammonia atmosphere at a crosslinking temperature ranging from room temperature to 400°C to obtain crosslinked infusible boron nitride precursor fibers, and then subjecting the fibers to a heat treatment to inorganicization and ceramicization to obtain the boron nitride fibers, wherein the low-concentration ammonia atmosphere is an atmosphere in which the ammonia concentration is lower than the ammonia concentration in the ammonia atmosphere.
[0009] The beneficial effects of the present invention by adopting the above technical solution are:
[0010] At low temperatures, the boron nitride precursor polyborazane reacts with ammonia mainly in the following ways:
[0011]
[0012] During the cross-linking process of boron nitride precursor fiber, ammonia mainly undergoes transamination (amine) reaction in the first step, where the amino group replaces the amino group on the boron nitride precursor fiber. However, when ammonia is present in large quantities, an aminolysis reaction will also occur, and the borane connecting the amino groups will be degraded by inserting the amino group, as shown in the above reaction process; in the second step, the generated amino group attacks other boron atoms and achieves cross-linking through deamination (amine). Ammonia atmosphere is conducive to the reaction in the first step, but not to the reaction in the second step; non-ammonia atmosphere is conducive to the reaction in the second step; therefore, an ammonia atmosphere is used to promote the transamination reaction to obtain a higher concentration of active amino groups. In order to avoid aminolysis, a non-ammonia atmosphere or a low-concentration ammonia atmosphere is introduced to promote the reaction in the second step to achieve cross-linking. Alternating treatment is performed to achieve efficient cross-linking of polyborazane, and an infusible precursor cross-linked fiber is obtained. The cross-linked fiber is then heat-treated to achieve inorganicization and ceramicization of the fiber, and a boron nitride fiber is prepared.
[0013] In summary, the technical innovation of the present invention lies in the alternating treatment of gases during the cross-linking process, that is, the alternating treatment of ammonia atmosphere and non-ammonia atmosphere or low-concentration ammonia atmosphere. As long as the non-ammonia atmosphere or low-concentration ammonia atmosphere can reduce the ammonia concentration in the second step reaction and inhibit ammonia decomposition, that is to say, as long as the gas atmosphere conditions of the above reaction are met, it will be fine.
[0014] Furthermore, the ammonia atmosphere is pure ammonia or a mixed gas atmosphere containing ammonia, and the volume fraction of ammonia in the mixed gas atmosphere is not less than 10%.
[0015] The beneficial effects of adopting the above further technical solution are:
[0016] In the ammonia atmosphere, the amine groups on the end groups and side chains of the boron nitride precursor fiber (polyborazane) are first replaced by amino groups, which easily attack the electron-deficient boron atoms to produce nucleophilic reactions and achieve cross-linking of the polyborazane.
[0017] Furthermore, the above-mentioned low-concentration ammonia atmosphere is a gas atmosphere in which the molar concentration of ammonia is not higher than 0.5 times the molar concentration of ammonia in the above-mentioned ammonia atmosphere.
[0018] Furthermore, the non-ammonia atmosphere is an inert gas atmosphere, a reactive gas atmosphere or a vacuum atmosphere.
[0019] What is meant here is that when the atmosphere alternation treatment is carried out, there are the following situations: alternating treatment of ammonia atmosphere (which can be pure ammonia or a mixture of ammonia and inert gas atmosphere, but the volume fraction of ammonia in the mixed gas is not less than 10%, and the ammonia atmospheres below are the same) and inert gas atmosphere; alternating treatment of ammonia atmosphere and active gas atmosphere; alternating treatment of ammonia atmosphere and vacuum atmosphere; alternating treatment of high-concentration ammonia atmosphere and low-concentration ammonia atmosphere.
[0020] Furthermore, the inert gas atmosphere is a gas that does not chemically react with the boron nitride precursor fiber at the crosslinking temperature; including but not limited to rare gases (such as argon, helium, etc.), nitrogen and hydrogen.
[0021] Furthermore, the active gas atmosphere is a gas that chemically reacts with the boron nitride precursor fiber at the crosslinking temperature; specifically, the active gas atmosphere is a pure gas of active gas or a mixed gas atmosphere containing such gas, and the active gas includes but is not limited to oxygen, oxidizing gases (such as nitrogen dioxide), boron compound gases (such as borane, boron halide, borazane, etc.) and silicon compound gases (such as silazane, silane, halosilanes and silicon halides, etc.), that is, it can be a single gas or a mixture of several gases among the above gases, or a mixed gas consisting of this single gas / gas mixture and an inert gas.
[0022] The beneficial effects of adopting the above further technical solution are:
[0023] After the ammonia atmosphere is used to promote the transamination reaction, a relatively high concentration of active amino groups is obtained. However, in the presence of a large amount of ammonia, polyborazane is easily aminolyzed to form volatile aminocyclic borazane. Therefore, after the amino groups have replaced the amino groups to a certain extent in the ammonia atmosphere, the ammonia concentration is reduced, that is, the above-mentioned non-ammonia atmosphere is used to reduce the ammonia concentration, inhibit the aminolysis of polyborazane, achieve efficient cross-linking, and improve the ceramic yield.
[0024] Furthermore, the cross-linking temperature is 50°C to 320°C.
[0025] The beneficial effects of adopting the above further technical solution are:
[0026] The mechanical properties of boron nitride fibers can be enhanced by subjecting boron nitride precursor fibers to atmosphere alternating treatment within a crosslinking temperature range of 50 to 320°C.
[0027] Furthermore, during the alternating treatment, at least one atmosphere other than the ammonia atmosphere is used alternately with the ammonia atmosphere; when performing the alternating treatment, the ammonia atmosphere can be used first, and then the non-ammonia atmosphere or low-concentration ammonia atmosphere can be used, or the non-ammonia atmosphere or low-concentration ammonia atmosphere can be used first and then the ammonia atmosphere can be used, and this process is not limited.
[0028] Furthermore, during the alternating treatment, the ammonia atmosphere and the non-ammonia atmosphere or the low-concentration ammonia atmosphere are alternated at least once.
[0029] In summary, the beneficial effects of the present invention are:
[0030] The present invention treats the boron nitride precursor fiber alternately with an ammonia atmosphere and a non-ammonia atmosphere or a low-concentration ammonia atmosphere during a heating process, so that the boron nitride precursor fiber is better cross-linked, and the ammonia decomposition thereof is avoided to produce volatile small molecules, and then the boron nitride fiber is prepared by heat treatment. The boron nitride fiber prepared by the method of the present invention can improve the ceramic yield, and the morphology of the prepared boron nitride fiber can reach a dense and non-hollow state, and the mechanical properties are also good. The tensile strength of the fiber can reach 1.3GPa, and the elastic modulus can reach 120GPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the morphology of boron nitride fiber. Specific embodiments
[0032] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0033] Example 1: Infusibility treatment with alternating ammonia atmosphere and inert atmosphere
[0034] A boron nitride fiber is prepared by the following steps:
[0035] The first step is precursor melt spinning: the precursor polyborazane is pre-heated in a melting kettle for melting, degassing, and de-sing, and then the material is spun through a spinneret with a hole diameter of 0.2 mm at a pressure of 1.5 MPa to obtain a precursor fiber with a diameter of 25 μm;
[0036] The second step is to make the precursor fiber infusible: the precursor fiber is placed in a closed container and cross-linked at a temperature range of 50°C to 320°C, with a heating rate of 0.5°C / min; two atmospheres are alternately treated, the first atmosphere is a mixture of nitrogen and ammonia (volume ratio of 1:1), and the second component is pure nitrogen, and the two atmospheres are switched every 10 minutes;
[0037] The third step is pyrolysis and inorganicization of the fiber: the fiber after the infusible treatment is further heated in an atmosphere of ammonia and nitrogen mixed gas (volume ratio of 1:1), from 300°C to 1000°C, with a heating rate of 1°C / min;
[0038] The fourth step is high temperature ceramicization of the fiber: the inorganic treated fiber is further heated up in a nitrogen atmosphere from 1000°C to 1600°C at a heating rate of 3°C / min.
[0039] The boron nitride fiber obtained by the above method has a tensile strength of 1.0 MPa and an elastic modulus of 98 GPa.
[0040] Example 2: Infusibility Treatment with Alternating Ammonia Atmosphere and Oxygen-Containing Atmosphere
[0041] A boron nitride fiber is prepared by the following steps:
[0042] The first step is precursor melt spinning: the precursor polyborazane is pre-heated in a melting kettle for melting, degassing, and de-sing, and then the material is spun through a spinneret with a hole diameter of 0.2 mm at a pressure of 1.5 MPa to obtain a precursor fiber with a diameter of 25 μm;
[0043] The second step is to make the precursor fiber infusible: the precursor fiber is placed in a closed container and cross-linked at a temperature range of 50°C to 320°C, wherein the heating rate is 0.5°C / min; two atmospheres are alternately treated, the first atmosphere is a mixture of nitrogen and ammonia (volume ratio is 1:1), and the second atmosphere is dry air (dry air contains oxygen, which is defined as oxygen in the active gas atmosphere), and the two atmospheres are switched every 10 minutes;
[0044] The third step is pyrolysis and inorganicization of the fiber: the fiber after the infusible treatment is further heated in an atmosphere of ammonia and nitrogen mixed gas (volume ratio of 1:1), from 300°C to 1000°C, with a heating rate of 1°C / min;
[0045] The fourth step is high temperature ceramicization of the fiber: the inorganic treated fiber is further heated up in a nitrogen atmosphere from 1000°C to 1600°C at a heating rate of 3°C / min.
[0046] The boron nitride fiber obtained by the above method has a tensile strength of 0.8 MPa and an elastic modulus of 115 GPa.
[0047] Example 3: Infusibility Treatment with Alternating Ammonia and Borane Atmospheres
[0048] A boron nitride fiber is prepared by the following steps:
[0049] The first step is precursor melt spinning: the precursor polyborazane is pre-heated in a melting kettle for melting, degassing, and de-sing, and then the material is spun through a spinneret with a pore size of 0.2 mm at a pressure of 1.5 MPa to obtain a precursor fiber with a diameter of 25 μm;
[0050] The second step is to make the precursor fiber infusible: the precursor fiber is placed in a closed container and cross-linked at a temperature range of 50°C to 320°C, wherein the heating rate is 0.5°C / min; two atmospheres are alternately treated, the first atmosphere is a mixture of nitrogen and ammonia (volume ratio is 1:1), and the second component is a mixture of diborane and nitrogen (the volume fraction of diborane is 2%); the procedure of the atmosphere alternation is 10 minutes of ammonia nitrogen mixture + 10 minutes of nitrogen + 10 minutes of diborane mixture + 10 minutes of nitrogen, and this cycle is carried out;
[0051] The third step is pyrolysis and inorganicization of the fiber: the fiber after the infusible treatment is further heated in an atmosphere of ammonia and nitrogen mixed gas (volume ratio of 1:1), from 300°C to 1000°C, with a heating rate of 1°C / min;
[0052] The fourth step is high temperature ceramicization of the fiber: the inorganic treated fiber is further heated up in a nitrogen atmosphere from 1000°C to 1600°C at a heating rate of 3°C / min.
[0053] The boron nitride fiber obtained by the above method has a tensile strength of 1.3 MPa and an elastic modulus of 120 GPa.
[0054] Comparative Example: Infusible Treatment in Ammonia Atmosphere
[0055] A boron nitride fiber is prepared by the following steps:
[0056] The first step is precursor melt spinning: the precursor polyborazane is pre-heated in a melting kettle for melting, degassing, and de-sing, and then the material is spun through a spinneret with a pore size of 0.2 mm at a pressure of 1.5 MPa to obtain a precursor fiber with a diameter of 25 μm;
[0057] The second step is to make the precursor fiber infusible: the precursor fiber is placed in a closed container and cross-linked at a temperature range of 50°C to 320°C, wherein the heating rate is 0.5°C / min; the atmosphere is a mixed gas of ammonia and nitrogen (volume ratio is 1:1);
[0058] The third step is pyrolysis and inorganicization of the fiber: the fiber after the infusible treatment is further heated in an atmosphere of ammonia and nitrogen mixed gas (volume ratio of 1:1), from 300°C to 1000°C, with a heating rate of 1°C / min;
[0059] The fourth step is high temperature ceramicization of the fiber: the inorganic treated fiber is further heated up in a nitrogen atmosphere from 1000°C to 1600°C at a heating rate of 3°C / min.
[0060] The boron nitride fiber obtained by the above method has a tensile strength of 0.5 MPa and an elastic modulus of 72 GPa.
[0061] The boron nitride fibers prepared in Examples 1-3 and the comparative example were compared and sorted, and the results are shown in Table 1.
[0062] Table 1 Effect of infusible treatment in different atmospheres on the prepared boron nitride fibers
[0063]
[0064] In the process of infusibility treatment of boron nitride precursor fibers in Examples 1-3 and the comparative example, different treatment methods are respectively adopted. It can be seen from the comparative example in Table 1 that when the boron nitride precursor is infusible, a mixed gas of ammonia and nitrogen (volume ratio is 1:1) is used for treatment, and it is not alternately treated with other non-ammonia atmospheres. The ceramic yield is low, hollowness exists in the final product, and the mechanical properties are poor. The boron nitride fibers obtained by alternating treatment with non-ammonia atmospheres and ammonia atmospheres are dense and free of hollowness, and the ceramic yield is high and the mechanical properties are good.
Claims
1. A chemical crosslinking method for preparing boron nitride fibers using an organic precursor method, It is characterized in that The following steps are involved: The boron nitride precursor fiber is subjected to alternating treatment in an ammonia atmosphere and a non-ammonia atmosphere or a low-concentration ammonia atmosphere at a crosslinking temperature ranging from room temperature to 400° C. to obtain a crosslinked infusible boron nitride precursor fiber, which is then subjected to a heat treatment to obtain a boron nitride fiber after inorganicization and ceramicization; The ammonia atmosphere is pure ammonia or a mixed gas atmosphere containing ammonia, and the volume fraction of ammonia in the mixed gas atmosphere is not less than 10%; The low-concentration ammonia atmosphere is a gas atmosphere in which the molar concentration of ammonia is not higher than 0.5 times the molar concentration of ammonia in the ammonia atmosphere; The non-ammonia atmosphere is an inert gas atmosphere or a vacuum atmosphere.
2. The chemical crosslinking method for preparing boron nitride fiber by organic precursor method according to claim 1, It is characterized in that The inert gas atmosphere is a gas that does not chemically react with the boron nitride precursor fiber at the crosslinking temperature.
3. The chemical crosslinking method for preparing boron nitride fiber by organic precursor method according to claim 1, It is characterized in that The cross-linking temperature is 50°C to 320°C.
4. The chemical crosslinking method for preparing boron nitride fiber by organic precursor method according to claim 1, It is characterized in that During the alternating treatment, the ammonia atmosphere and the non-ammonia atmosphere or the low-concentration ammonia atmosphere are alternated at least once.