Fiber-reinforced slag-bagasse ash-based geopolymer material and preparation method thereof

By replacing cement with slag and bagasse ash and combining fiber reinforcement technology, a low-carbon and environmentally friendly fiber-reinforced slag-sugar cane bagasse ash-based geological polymer material is prepared, which solves the high energy consumption and high carbon fiber-reinforced cement-based composite materials. The emission issues have achieved low-carbon, environmentally friendly and high-performance materials.

CN116143457BActive Publication Date: 2024-11-19GUANGXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310058382.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-11-19
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

The existing fiber-reinforced cement-based composites have high energy consumption and high carbon emissions during the production process, and there is a lack of green materials that can replace cement to achieve their greening.

Method used

Develop a fiber-reinforced slag-bag ash-based geological polymer material composed of slag, bagasse ash, fine sand, water glass, fiber, sodium hydroxide, water reducer and retarder, through specific proportions and treatments Methods to prepare this material completely replace cement.

Benefits of technology

It has achieved low-carbon and environmentally friendly, low-priced, high early strength, high extreme tensile strain, excellent compression and flexural resistance, and meets the needs of greening and high performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004060858850000031
    Figure BDA0004060858850000031
  • Figure BDA0004060858850000041
    Figure BDA0004060858850000041
  • Figure HDA0004060858860000011
    Figure HDA0004060858860000011
Patent Text Reader

Abstract

The present invention belongs to the field of composite concrete materials, and discloses a fiber-reinforced slag-bagasse ash-based geopolymer material and a preparation method thereof, wherein the composite material is prepared by mixing slag, bagasse ash, fine sand, fiber, water glass, sodium hydroxide, water reducer, retarder and water, wherein the total mass percentage of slag, bagasse ash, fine sand, fiber, water glass, sodium hydroxide, water reducer and retarder is 90.7%-91.7%, and the mass percentage of water is 8.3%-9.3%. The cementitious material of the fiber-reinforced slag-bagasse ash-based geopolymer material of the present invention uses slag and bagasse ash in its entirety, and has the significant advantages of low carbon, environmental protection and low price compared with traditional cement-based materials, and has both high strength and good ductility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a fiber-reinforced slag-bagasse ash-based geopolymer material and a preparation method thereof. Background Art

[0002] Fiber-reinforced cementitious composites (ECC) have been developed as a special type of fiber-reinforced concrete. They have ultra-high ductility and a strain capacity that is hundreds of times greater than that of ordinary concrete, overcoming the shortcomings of traditional concrete's insufficient tensile deformation capacity. The tensile deformation of fiber-reinforced cementitious composites develops from cracking at the initial crack point to multiple cracks in the entire specimen, and produces a large number of microcracks with a width of less than 100um, which can effectively prevent harmful substances from penetrating too quickly and causing damage.

[0003] It is particularly important to promote the greening of fiber-reinforced cement-based composite materials, especially low energy consumption and low carbon emissions. Fiber-reinforced cement-based composite materials do not contain coarse aggregates, resulting in a higher cement content than ordinary concrete. In addition, since cement production is a high-energy consumption industry, a large amount of carbon dioxide will be emitted during the process, which will bring serious burdens to the environment.

[0004] One of the main ways to achieve green ECC is to screen out green materials that can replace cement. Industrial and agricultural wastes have great potential due to their low cost and high material liquidity. In the process of screening materials, the main focus is on mechanical factors, chemical characteristics and material sustainability. Therefore, the development of a low-carbon, high-strength, high-ductility fiber-reinforced slag-bagasse ash-based geopolymer material has good prospects. Summary of the invention

[0005] In view of the above problems, the present invention provides a fiber reinforced slag-bagasse ash-based geopolymer material with easily available raw materials, low cost, high strength and good toughness, and a preparation method thereof.

[0006] To achieve the above object, the technical solution of the present invention is to provide a fiber-reinforced slag-bagasse ash-based geopolymer material, wherein the polymer material is mixed with slag, bagasse ash, fine sand, water glass, fiber, sodium hydroxide, water reducer, retarder and water, wherein the total mass percentage of slag, bagasse ash, fine sand, water glass, fiber, sodium hydroxide, water reducer and retarder is 90.7%-91.7%, and the mass percentage of water is 8.3%-9.3%.

[0007] The specific composition and weight ratio are: 31%-41% slag, 11%-21% bagasse ash, 21% fine sand, 14% water glass, 1.1% fiber, 1.6% sodium hydroxide, 0.5%-1% water reducer, 0.5%-1% retarder, and 8.3%-9.3% water.

[0008] The slag is S95 grade slag powder. The fine sand is 150-200 mesh quartz sand.

[0009] The fiber is polyvinyl alcohol fiber, with a fiber length of 12 mm and a fiber diameter of 39 μm.

[0010] The water glass has a modulus of 2.3, a silicon dioxide content of 30 wt.%, and a sodium oxide content of 13.5 wt.%.

[0011] The purity of the sodium hydroxide is greater than 96%. The water reducer is a polycarboxylic acid, and the retarder is barium chloride dihydrate.

[0012] The bagasse ash is pre-treated by calcining at 600° C. for 2 hours in an industrial combustion furnace and then grinding in a ball mill for 3 hours. The particle size of the calcined and ground bagasse ash is in the range of 5-100 μm.

[0013] The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material comprises the following steps:

[0014] (1) dissolving sodium hydroxide in water glass and mixing it evenly by ultrasonication for 30 min, and then standing at room temperature for use;

[0015] (2) adding slag, bagasse ash and fine sand in weight ratios of 31%-41%, 11%-21% and 21% to the mortar in turn and dry mixing for 30 seconds to ensure that the base materials are evenly mixed;

[0016] (3) uniformly mixing a retarder with a weight ratio of 0.5%-1% and 8.3%-9.3% with water and adding the above-mentioned base material, and adding the pre-prepared alkali activator and stirring for 30 seconds to form a paste slurry;

[0017] (4) Add 0.5%-1% water reducer by weight, stir slowly for 30 seconds and then stir quickly for 60 seconds;

[0018] (5) Add 1.1% by weight of fiber and continue to stir rapidly for 5 minutes until the fiber is evenly dispersed to obtain a fiber-reinforced slag-bagasse ash-based geopolymer material.

[0019] The present invention has the following beneficial effects:

[0020] 1. Low carbon, environmentally friendly and low price

[0021] The present invention uses slag and bagasse ash to completely replace cement. Slag is an industrial byproduct; bagasse ash is a waste product from burning sugarcane and does not require additional purchase costs; therefore, the present invention has the significant advantages of low carbon, environmental protection and low price.

[0022] 2. High ductility

[0023] The 28-day ultimate tensile strain of the fiber-reinforced slag-bagasse ash-based geopolymer material used in the present invention reaches 5%-7%, far exceeding the 3% ultimate tensile strain requirement specified for ECC materials.

[0024] 3. High early strength

[0025] The fiber-reinforced slag-bagasse ash-based geopolymer material used in the present invention can achieve a one-day compressive strength of more than 50 MPa and a one-day flexural strength of more than 10 MPa, and has a significant advantage of high early strength.

[0026] 4. Good compression and bending resistance

[0027] The fiber-reinforced slag-bagasse ash-based geopolymer material designed by the present invention has the characteristics of low carbon and environmental protection, high toughness, and high early strength, and also has good 28-day compressive and flexural strength. Since slag and bagasse ash are selected as the base material of the matrix, and the fiber has a bridging effect on cracks, the material has excellent compressive and flexural properties. By adjusting the bagasse ash mix ratio, the 28d compressive strength of the material reaches 75-85MPa, and the flexural strength reaches more than 10MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a flow chart of the preparation method of the fiber reinforced slag-bagasse ash-based geopolymer material of the present invention. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described in detail below in conjunction with embodiments.

[0030] Example 1

[0031] This embodiment is an example of the fiber-reinforced slag-bagasse ash-based geopolymer material described in the present invention, which includes the following raw materials in proportion by mass: 41% slag; 11% bagasse ash; 21% fine sand; 14% water glass; 1.1% fiber; 1.6% sodium hydroxide; 1% water reducer; 1% retarder; and 8.3% water.

[0032] The slag is S95 grade slag powder; bagasse ash is calcined at 600°C for 2 hours and then ground in a ball mill for 3 hours, and its particle size is 5-100μm; the fine sand is quartz sand with a mesh size of 150-200; the water glass modulus is 2.3, the silicon dioxide content is 30wt.%, and the sodium oxide content is 13.5wt.%; the fiber is polyvinyl alcohol fiber, the fiber length is 12mm, and the fiber diameter is 39μm; the purity of sodium hydroxide is greater than 96%; the water reducer and the retarder are polycarboxylic acid water reducer and barium chloride dihydrate respectively.

[0033] The preparation method of the fiber-reinforced slag-bagasse ash-based geopolymer material is as follows: 14% and 1.6% of water glass and sodium hydroxide are evenly mixed 24 hours in advance as an alkali activator for standby use; slag, bagasse ash and fine sand with a weight ratio of 41%, 11% and 21% are sequentially added to a mortar mixer and dry-mixed for 30 seconds to make each matrix material evenly mixed; then, a retarder with a weight ratio of 1% and 8.3% is evenly mixed with water and added to the above-mentioned matrix material, and the alkali activator prepared in advance is added and continued to be stirred, and a paste slurry is formed after slow stirring for 30 seconds; then a water reducer with a weight ratio of 1% is added, and it is slowly stirred for 30 seconds and then quickly stirred for 60 seconds until the slurry has good fluidity; finally, fiber with a weight ratio of 1.1% is added, and stirring is continued for 5 minutes until the fiber is evenly dispersed to obtain the fiber-reinforced slag-bagasse ash-based geopolymer material.

[0034] The test results of various performance tests of the product obtained in this case are listed in Table 1. Among them, the test blocks used for mechanical tests were demoulded for 24 hours and placed in a standard curing room with a temperature of 20±2℃ and a humidity of 90±5℃ for curing. After 28 days, compression and flexural tests were carried out on a universal testing machine. The uniaxial tensile test was carried out using a special dog-bone-shaped test block and a 10-ton universal testing machine. The loading speed was 0.5mm / min, and the tensile strain was measured using LVDT.

[0035] Table 1 Test results of implementation case 1 environmentally friendly high-strength and high-ductility fiber-reinforced alkali-activated slag-bagasse ash-based polymer materials

[0036]

[0037] Example 2

[0038] This embodiment is another example of the fiber-reinforced slag-bagasse ash-based geopolymer material described in the present invention, which includes the following raw materials in proportion by mass: 31% slag; 21% bagasse ash; 21% fine sand; 14% water glass; 1.1% fiber; 1.6% sodium hydroxide; 0.5% water reducer; 0.5% retarder; and 9.3% water.

[0039] The slag is S95 grade slag powder; bagasse ash is calcined at 600°C for 2 hours and then ground in a ball mill for 3 hours, and its particle size is 5-100μm; the fine sand is quartz sand with a mesh size of 150-200; the water glass modulus is 2.3, the silicon dioxide content is 30wt.%, and the sodium oxide content is 13.5wt.%; the fiber is polyvinyl alcohol fiber, the fiber length is 12mm, and the fiber diameter is 39μm; the purity of sodium hydroxide is greater than 96%; the water reducer and the retarder are polycarboxylic acid water reducer and barium chloride dihydrate respectively.

[0040] The preparation method of the above-mentioned fiber reinforced slag-bagasse ash-based geopolymer material is as follows: 14% and 1.6% of water glass and sodium hydroxide are mixed evenly 24 hours in advance as an alkali activator for standby use; slag, bagasse ash and fine sand with a weight ratio of 31%, 21% and 21% are added to a mortar mixer in turn and dry mixed for 30 seconds until each matrix material is mixed evenly; then, a retarder with a weight ratio of 0.5% and 9.3% is evenly mixed with water and added to the above-mentioned matrix material, and the alkali activator prepared in advance is added and continued to be slowly stirred for 30 seconds until a paste slurry is formed; then a water reducer with a weight ratio of 0.5% is added, and it is slowly stirred for 30 seconds and then quickly stirred for 60 seconds until the slurry has good fluidity; finally, fiber with a weight ratio of 1.1% is added and stirred for 5 minutes until the fiber is evenly dispersed to obtain a fiber reinforced slag-bagasse ash-based geopolymer material.

[0041] The test results of various performance tests of the product obtained in this case are listed in Table 2. Among them, the test blocks used in the mechanical test were demoulded for 24 hours and placed in a standard curing room with a temperature of 20±2℃ and a humidity of 90±5℃ for curing. After 28 days, compression and flexural tests were carried out on a universal testing machine. The uniaxial tensile test was carried out using a special dog-bone-shaped test block and a 10-ton universal testing machine. The loading speed was 0.5mm / min, and the tensile strain was measured using LVDT.

[0042] Table 2 Test results of implementation case 2 environmentally friendly high-strength and high-ductility fiber reinforced alkali-activated slag-bagasse ash-based composite materials

[0043]

Claims

1. A method for preparing a fiber-reinforced slag-bagasse ash-based geopolymer material, characterized in that: The specific composition and weight ratio of the polymer material are: 31%-41% slag, 11%-21% bagasse ash, 21% fine sand, 14% water glass, 1.1% fiber, 1.6% sodium hydroxide, 0.5%-1% water reducer, 0.5%-1% retarder, and 8.3%-9.3% water; The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material comprises the following steps: (1) Dissolve sodium hydroxide in water glass and mix it evenly by ultrasonication for 30 min, then let it stand at room temperature for use; (2) Add slag, bagasse ash and fine sand with a weight ratio of 31%-41%, 11%-21% and 21% to the mortar in sequence and dry mix for 30 seconds to ensure that the base materials are evenly mixed; (3) Evenly mix the retarder with water in a weight ratio of 0.5%-1% and 8.3%-9.3% and add it to the above-mentioned base material. At the same time, add the alkali activator prepared in advance and continue stirring for 30 seconds to form a paste slurry; (4) Add 0.5%-1% water reducer by weight, stir slowly for 30 seconds and then stir quickly for 60 seconds; (5) Add 1.1% fiber by weight and continue to stir rapidly for 5 min until the fibers are evenly dispersed to obtain a fiber-reinforced slag-bagasse ash-based geopolymer material. The 28-day compressive strength of the material is 75-85 MPa, and the flexural strength is above 10 MPa.

2. The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material according to claim 1, characterized in that: The slag is S95 grade slag powder.

3. The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material according to claim 1, characterized in that: The fine sand is 150-200 mesh quartz sand.

4. The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material according to claim 1, characterized in that: The fiber is polyvinyl alcohol fiber, with a fiber length of 12 mm and a fiber diameter of 39 μm.

5. The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material according to claim 1, characterized in that: The water glass has a modulus of 2.3, a silicon dioxide content of 30 wt.%, and a sodium oxide content of 13.5 wt.%.

6. The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material according to claim 1, characterized in that: The sodium hydroxide purity is greater than 96%.

7. The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material according to claim 1, characterized in that: The water reducing agent is polycarboxylic acid, and the retarder is barium chloride dihydrate.

8. The method for preparing the fiber-reinforced slag-bagasse ash-based geopolymer material according to claim 1, characterized in that: The bagasse ash is pre-treated by calcining at 600° C. for 2 h in an industrial combustion furnace and then grinding in a ball mill for 3 h. The particle size of the calcined and ground bagasse ash ranges from 5 to 100 μm.