A gadolinium-based nanofluorine cluster for magnetic refrigeration and a preparation method thereof
By preparing gadolinium-based fluorine nanoclusters, the problem of decreasing magnetic entropy in existing magnetic refrigeration materials has been solved, achieving efficient and stable low-temperature magnetic refrigeration, applicable to the temperature range of 0.3K to 40K, and is environmentally friendly.
Patent Information
- Application Number
- CN202310184704.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-28
AI Technical Summary
Existing magnetic refrigeration materials have small magnetic entropy changes, which cannot meet the requirements of high-efficiency refrigeration, and traditional liquid refrigerants are harmful to the environment.
By using gadolinium-based fluorine nanoclusters, the structure Gd16(μ4-F)6(μ3-F)12[(CH3)3CCOO]18[N(CH2CH2O)3]4 was synthesized via a solvothermal reaction. Zero-dimensional nanomaterials were formed by fluorine ion bridging and encapsulation with trimethylacetic acid and triethanolamine to avoid rare earth ions being exposed to organic solvents, thus preparing a magnetic working material with high magnetic entropy change.
It achieves high-efficiency low-temperature magnetic refrigeration performance, has good material stability, is environmentally friendly, has no fluorine emissions, has a large magnetic entropy change value, and is suitable for a temperature range of 0.3K to 40K.
Smart Images

Figure CN116143810B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material science, and particularly relates to a gadolinium-based nano-fluorine cluster for magnetic refrigeration and a preparation method thereof. Background Art
[0002] Cryogenic refrigeration refers to refrigeration technology with a refrigeration temperature below 120K. The key steps are the cooling of the refrigerant, the absorption of heat from the object being cooled, and the release of heat. Liquid evaporative refrigeration, as one of the traditional cryogenic refrigeration technologies, is widely used in many industries such as petrochemicals, light industry and medicine, refrigeration and air conditioning, food refrigeration, national defense and aerospace; but the large-scale use of liquid refrigerants such as chlorofluorocarbons, chlorofluorocarbons and liquid hydrofluorocarbons has led to ozone depletion and greenhouse effects, and has become a globally banned environmental hazard. In addition, the lowest liquefaction temperature that this technology can achieve is about 2K (liquid helium-3), which cannot meet the needs of today's cutting-edge scientific research and the development of high-tech.
[0003] In order to solve the above-mentioned problems, environmentally friendly, energy-saving and efficient magnetic refrigeration technology provides a solution. By changing the strength of the external magnetic field, the magnetic moment of the material changes, so that the magnet absorbs and releases heat. The operating temperature of this technology can be from room temperature to below 1K. The magnetic working fluid usually selects a magnet with a large magnetic entropy change under a low magnetic field. Since this type of material is solid and has an entropy density much greater than that of a gaseous refrigerant, the volume of the refrigeration equipment can be significantly reduced. For example, a Chinese patent with publication number CN111403137A discloses a rare earth RE2ZnMnO6 oxide magnetic refrigeration material and a preparation method thereof. A simple and easy sol-gel method is used to synthesize a material with low-temperature magnetic refrigeration properties; as an important indicator for measuring its refrigeration effect, the maximum isothermal magnetic entropy change of the material is only 25.26 J·Kg -1 ·K -1 , its magnetic refrigeration performance is poor and cannot meet the current refrigeration needs.
[0004] According to the Maxwell relation of magnetic media, the magnetic entropy change is proportional to the spin value, so a large spin value is required to obtain high-performance magnetic refrigeration materials. Among the 17 rare earth ions, gadolinium ions have isotropic electron orbits, weak magnetic interactions, and high spin values generated by seven electrons on their 4f electron layer, which makes gadolinium-based compounds show good magnetic refrigeration properties. At present, the research on gadolinium-based compound materials is mainly focused on hydroxyl-bridged clusters, and the number of cluster nuclei, bridging atoms, and the types of organic ligands are all important factors affecting the magnetic exchange effect. Therefore, constructing novel gadolinium-based molecular clusters and exploring their magnetocaloric effects at low temperatures to obtain high-performance magnetic refrigeration materials has become a key issue that needs to be solved urgently. Summary of the invention
[0005] The purpose of the present invention is to provide a gadolinium-based nanofluorine cluster for magnetic refrigeration and a preparation method thereof to overcome the deficiencies of the prior art. The present invention can effectively improve low-temperature magnetic entropy change.
[0006] A gadolinium-based nanofluorine cluster for magnetic refrigeration, the molecular formula of the structure is Gd 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4, μ4-F and μ3-F are bridging modes of fluoride ions, (CH3)3CCOOH is trimethylacetic acid, and N(CH2CH2OH)3 is triethanolamine.
[0007] Preferably, the gadolinium-based fluorine-bridged cluster is a zero-dimensional nano-sized material.
[0008] Preferably, the application temperature of the gadolinium-based fluorine-bridged cluster magnetic refrigeration material is 0.3K to 40K.
[0009] Preferably, the magnetic field applied in the magnetization stage is 0.5T to 7T.
[0010] A method for preparing gadolinium-based nano-fluorine clusters for magnetic refrigeration comprises the following steps:
[0011] S1, dissolving and dispersing a rare earth precursor, a ligand and a deprotonated base in an organic solvent to obtain a solution A;
[0012] S2, dispersing the fluorine source in ethanol to obtain solution B, mixing solution A and solution B evenly and then performing a solvothermal reaction, and obtaining a colorless and transparent gadolinium-based fluorine-bridged cluster magnetic refrigeration crystal material by programmed cooling.
[0013] Preferably, the fluorine source is one of triethylamine trihydrofluoride, ammonium fluoride, tetramethylammonium fluoride tetrahydrate or sodium fluoride.
[0014] Preferably, the organic solvent is one or a mixture of N,N-dimethylformamide, acetonitrile, anhydrous methanol or ethanol.
[0015] Preferably, the rare earth precursor is gadolinium trimethylacetate.
[0016] Preferably, the solvent thermal reaction temperature is 120-160° C., the reaction time is 24-72 hours, and the programmed cooling rate is 3-10 degrees Celsius per hour.
[0017] Preferably, the molar ratio of the rare earth precursor, triethanolamine, triethylamine and fluorine source is 1:0.1-3:0.1-3:0.5-3.
[0018] Compared with the prior art, the present invention has the following beneficial technical effects:
[0019] The invention discloses a gadolinium-based nano-fluorine cluster for magnetic refrigeration, which has a simple preparation process, can obtain a pure sample under the condition of solvent thermal reaction, is simple to subsequently process with high yield, and is easy to enrich; the material has good corrosion resistance and is easy to process and form, and has good thermal stability so that it can stably exist at 450 degrees Celsius; the introduction of fluorine ions in the structure enables weaker antiferromagnetic exchange between gadolinium ions, and shows a large magnetic entropy change under low temperature and low field, and is an ideal magnetic working fluid for realizing low-temperature magnetic refrigeration.
[0020] The invention discloses a method for preparing gadolinium-based nano-fluorine clusters for magnetic refrigeration. The method comprises reacting a fluorine source that is not easily soluble in an organic solvent with a binuclear rare earth precursor, thereby avoiding direct exposure of rare earth ions to an organic solvent. In the process, no insoluble gadolinium fluoride precipitate is generated. By regulating the ratio of reactants and a deprotonating agent, triethylamine, a colorless and transparent block crystal of a gadolinium-based nano-fluorine cluster with a complete reaction and a pure phase is obtained. The periphery of the structure is completely wrapped by trimethylacetic acid and triethanolamine without solvent coordination, and the crystal has good thermal stability and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is the Gd in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Crystal structure diagram of [N(CH2CH2O)3]4;
[0022] Figure 2 is the Gd in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Space filling pattern diagram of [N(CH2CH2O)3]4 molecule;
[0023] Figure 3 is the Gd in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Temperature-dependent magnetic susceptibility curve of [N(CH2CH2O)3]4 under an external magnetic field of 1000Oe;
[0024] Figure 4 is the Gd in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The curve of the inverse of the molar magnetic susceptibility of [N(CH2CH2O)3]4 in an external magnetic field of 1000Oe versus temperature;
[0025] Figure 5is the Gd in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 A graph showing the relationship between the magnetization intensity of [N(CH2CH2O)3]4 and the magnetic field strength at different temperatures.
[0026] Figure 6 is the Gd in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Magnetic entropy change curve of [N(CH2CH2O)3]4 at different temperatures.
[0027] Figure 7 is the Gd in Example 1 of the present invention 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Mass spectrum of [N(CH2CH2O)3]4 in organic solvent tetrahydrofuran. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0029] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0030] The invention provides a gadolinium-based nanofluorine cluster for magnetic refrigeration, the molecular formula of which is Gd 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18[N(CH2CH2O)3]4, where μ4-F and μ3-F are two bridging modes of fluoride ions, (CH3)3CCOOH is trimethylacetic acid, [(CH3)3CCOO] - is trimethylacetate ion, N(CH2CH2OH)3 is triethanolamine, [N(CH2CH2O)3] 3- It is a completely deprotonated triethanolamine ion; the gadolinium-based nanofluorine cluster is a zero-dimensional nanomaterial. The gadolinium-based nanofluorine cluster used for magnetic refrigeration in the present application can achieve the magnetic working medium of ultra-low temperature refrigeration, has high refrigeration efficiency, is environmentally friendly and has no fluorine emissions.
[0031] A method for preparing gadolinium-based nano-fluorine clusters for magnetic refrigeration comprises the following steps:
[0032] S1, dissolving and dispersing a rare earth precursor, a ligand and a deprotonated base in an organic solvent to obtain a solution A;
[0033] S2, dispersing the fluorine source in ethanol to obtain solution B, mixing solution A and solution B, performing a solvothermal reaction, and obtaining colorless and transparent gadolinium-based nanofluorine clusters by programmed cooling.
[0034] The molar ratio of the rare earth precursor, triethanolamine, triethylamine and fluorine source is 1:0.1-3:0.1-3:0.5-3.
[0035] The ethanol is anhydrous ethanol. Solution A and solution B are mixed and placed in polytetrafluoroethylene for solvent thermal reaction. Polytetrafluoroethylene is a special reaction container for high-pressure reactors, which is resistant to acid and alkali, high temperature and high pressure.
[0036] The solvent thermal reaction temperature is 120-160°C, the reaction time is 24-72 hours, and the programmed cooling rate is 3-10°C per hour.
[0037] The fluorine source is one of triethylamine trihydrofluoride, ammonium fluoride, tetramethylammonium fluoride tetrahydrate or sodium fluoride.
[0038] The organic solvent is one or a mixture of N,N-dimethylformamide, acetonitrile, anhydrous methanol or ethanol.
[0039] The rare earth precursor is trimethylacetate rare earth salt, specifically gadolinium trimethylacetate.
[0040] The ligand is a tridentate alcoholamine ligand, specifically triethanolamine; and the deprotonated base is specifically triethylamine.
[0041] The prepared gadolinium-based nanofluorine cluster crystals for magnetic refrigeration belong to the orthorhombic crystal system with a space group of Pbcm.
[0042] The present application uses a mixed solvent of N,N-dimethylformamide, acetonitrile and ethanol, which can greatly improve the yield and make the solubility of the reactants moderate, which is the best environment for product crystallization; while methanol and ethanol mixed solvents easily dissolve the reactants, resulting in difficulty in precipitation of crystals and a lower yield.
[0043] According to the formula -ΔS M =nRln(2s+1), it can be seen that the magnetic entropy change value is determined by the number of nuclei and spin values of the rare earth gadolinium ions. The radius of the fluorine ion is smaller than that of the hydroxide. The gadolinium clusters bridged by hydroxyl groups are usually antiferromagnetic exchange interactions, while the gadolinium clusters bridged by fluorine groups are theoretically ferromagnetic exchange interactions. The ferromagnetic exchange interaction can make its spin value s larger and closer to the ideal value 7 / 2. The magnetic exchange of this material is mainly determined by two fluorine bridging modes μ4-F and μ3-F: when the Gd-F-Gd bond angle is an acute angle, it is an antiferromagnetic exchange interaction, such as the μ4-F bridging mode; combined with the magnetic characterization results, it shows that the material is a weak antiferromagnetic exchange interaction. In addition, since the number of rare earth gadolinium ion nuclei N in the structure is 16, the total maximum magnetic entropy change is large, showing excellent magnetic refrigeration performance.
[0044] The specific embodiments of the present invention are as follows:
[0045] Example 1
[0046] 0.5 mmol of trimethyl gadolinium acetate, 0.25 mmol of triethanolamine and 0.75 mmol of triethylamine were weighed and placed in a beaker, and added to a mixture of 3 ml of acetonitrile and 4 ml of N, N-dimethylformamide to completely dissolve the mixture to obtain solution A; in another beaker, 1 mmol of amine fluoride and 2 ml of ethanol were added and stirred to disperse the mixture to obtain solution B; solution A and solution B were mixed and poured into a 15 ml polytetrafluoroethylene bottle, and reacted in a temperature-controlled oven at 160° C. for 72 hours, and cooled to room temperature after 36 hours to obtain pure colorless block crystals, and the molecular structure thereof was determined to be Gd by single crystal X-ray diffractometer. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4; washed three times with acetonitrile and dried, yield 75%.
[0047] Figure 1 Gd 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Schematic diagram of the structure of the [N(CH2CH2O)3]4 molecule (H atoms are omitted in the figure), showing the spatial arrangement of 16 gadolinium ions, with every seven gadolinium ions sharing one face, and two adjacent faces sharing two gadolinium ions. There are a total of 18 bridging fluoride ions and 4 completely deprotonated triethanolamines involved in the coordination; Figure 2 Gd 16(μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 Space-filling pattern diagram of the [N(CH2CH2O)3]4 molecule. The measured size of the molecule is approximately 2nm×2nm. Figure 3 Gd 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The temperature-dependent magnetic susceptibility curve of [N(CH2CH2O)3]4 under an external magnetic field of 1000Oe shows that the χT value of the sample is 125.63cm at room temperature 300K. 3 Kmol -1 , which is slightly smaller than the theoretical value for 16 non-interacting gadolinium ions. Figure 4 Gd 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The curve of the inverse of the molar magnetic susceptibility of [N(CH2CH2O)3]4 under an external magnetic field of 100000e versus temperature shows that the gadolinium ions in the sample have a weak antiferromagnetic exchange interaction, and the Curie constant is 126.1 cm 3 mol -3 K, the Weiss constant is -0.79K. Figure 5 Gd 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 The relationship between the magnetization intensity of [N(CH2CH2O)3]4 and the magnetic field strength at different temperatures. The magnetization intensity reaches the saturation value of 111.6μ at 2K temperature and 7T magnetic field. B . See Figure 6 As the temperature decreases, the magnetic entropy change gradually increases. At a temperature of 2.5K, the magnetic entropy change under a 2T magnetic field is 20.7J·kg -1 K -1 ; The magnetic entropy change under 1.5T magnetic field is 14.6J·kg -1 ·K -1 ; The magnetic entropy change under 1T magnetic field is 8.0J·kg -1 K -1 ; The magnetic entropy change under 0.5T magnetic field is 2.3J·kg -1 ·K -1 . Figure 7 Display Gd 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18The [N(CH2CH2O)3]4 sample has good stability in tetrahydrofuran solution. The mass spectrometry result differs from the molecular formula obtained by single crystal analysis by 19, that is, one fluoride ion with a molecular weight of 5262.032, which verifies that the sample molecular cluster contains 18 fluoride ions.
[0048] By analyzing the magnetic entropy change of fluorine-bridged rare earth clusters in low temperature and low field regions, it was found that in a magnetic field environment of 1 to 3 T, the curve rises sharply as the temperature decreases, and no peak appears. In a higher magnetic field, it shows a gentler upward trend. That is, in a low field environment, the magnetic refrigeration performance of this material is better than most previously known gadolinium-based molecular clusters, showing an excellent magnetocaloric effect and is suitable for low temperature regions.
[0049] Example 2
[0050] 0.5 mmol of trimethyl gadolinium acetate, 0.25 mmol of triethanolamine and 0.75 mmol of triethylamine were weighed into a beaker, and 3 ml of acetonitrile and 4 ml of N, N-dimethylformamide were added to dissolve them completely; 0.161 g (1 mmol) of triethylamine trihydrofluoride and 2 ml of ethanol were added to another beaker and mixed evenly; the two solutions were mixed and poured into a 15 ml polytetrafluoroethylene bottle, reacted in a temperature-controlled oven at 120° C. for 24 hours, and cooled to room temperature after 40 hours to obtain pure colorless block crystals, and the molecular structure thereof was determined to be Gd by single crystal X-ray diffractometer. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4; washed three times with acetonitrile and dried, yield 41%.
[0051] Example 3
[0052] 1 mmol of trimethyl gadolinium acetate, 0.5 mmol of triethanolamine and 1.5 mmol of triethylamine were weighed into a beaker, and 3 ml of acetonitrile and 4 ml of N, N-dimethylformamide were added to dissolve them completely; 0.074 g (2 mmol) of amine fluoride and 2 ml of ethanol were added to another beaker and stirred to disperse; the two solutions were mixed and poured into a 15 ml polytetrafluoroethylene bottle, reacted in a temperature-controlled oven at 150° C. for 72 hours, and cooled to room temperature after 40 hours to obtain pure colorless block crystals, and the molecular structure thereof was determined to be Gd by single crystal X-ray diffractometer. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4; washed three times with acetonitrile and dried, yield 79%.
[0053] Example 4
[0054] Weigh 1 mmol of trimethyl gadolinium acetate, 0.5 mmol of triethanolamine and 1.5 mmol of triethylamine in a beaker, add 7 ml of anhydrous methanol to dissolve them completely; take another beaker, add 0.074 g (2 mmol) of amine fluoride and 2 ml of ethanol and stir to disperse; mix the above two solutions and pour them into a 15 ml polytetrafluoroethylene bottle, react in a temperature-controlled oven at 150° C. for 72 hours, cool to room temperature after 40 hours to obtain pure colorless transparent rod-shaped crystals, and determine its molecular structure to be Gd by single crystal X-ray diffractometer. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4; washed three times with acetonitrile and dried, yield 63%.
[0055] Example 5
[0056] Weigh 1 mmol of trimethyl gadolinium acetate, 0.5 mmol of triethanolamine and 1.5 mmol of triethylamine in a beaker, add 7 ml of anhydrous methanol to dissolve them completely; take another beaker, add 0.074 g (2 mmol) of amine fluoride and 2 ml of ethanol and stir to disperse; mix the above two solutions and pour them into a 15 ml polytetrafluoroethylene bottle, react in a temperature-controlled oven at 120° C. for 48 hours, cool to room temperature after 24 hours to obtain pure colorless transparent rod-shaped crystals, and determine its molecular structure to be Gd by single crystal X-ray diffractometer. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4; washed three times with acetonitrile and dried, yield 45%.
[0057] Example 6
[0058] 0.5 mmol of trimethyl gadolinium acetate, 0.25 mmol of triethanolamine and 0.75 mmol of triethylamine were weighed into a beaker, and 7 ml of anhydrous methanol was added to dissolve them completely; 0.037 g (1 mmol) of amine fluoride and 2 ml of ethanol were added to another beaker and stirred to disperse; the above two solutions were mixed and poured into a 15 ml polytetrafluoroethylene bottle, reacted in a temperature-controlled oven at 150° C. for 72 hours, and cooled to room temperature after 36 hours to obtain pure colorless block crystals, and the molecular structure thereof was determined to be Gd by single crystal X-ray diffractometer. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4; washed three times with acetonitrile and dried, yield 51%.
[0059] Example 7
[0060] 1 mmol of trimethyl gadolinium acetate, 0.1 mmol of triethanolamine and 0.1 mmol of triethylamine were weighed into a beaker, and 3 ml of acetonitrile and 4 ml of N, N-dimethylformamide were added to dissolve them completely; 0.004 g (0.1 mmol) of amine fluoride and 2 ml of ethanol were added to another beaker and stirred to disperse; the above two solutions were mixed and poured into a 15 ml polytetrafluoroethylene bottle, reacted in a temperature-controlled oven at 150° C. for 72 hours, and cooled to room temperature after 36 hours to obtain pure colorless block crystals, and the molecular structure thereof was determined to be Gd by single crystal X-ray diffractometer. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4; washed three times with acetonitrile and dried, yield 9%.
[0061] Example 8
[0062] Weigh 1 mmol of trimethyl gadolinium acetate, 3 mmol of triethanolamine and 3 mmol of triethylamine in a beaker, add 3 ml of acetonitrile and 4 ml of N,N-dimethylformamide to dissolve them completely; take another beaker, add 0.111 g (3 mmol) of amine fluoride and 2 ml of ethanol and stir to disperse; mix the above two solutions and pour them into a 15 ml polytetrafluoroethylene bottle, react in a temperature-controlled oven at 150° C. for 72 hours, cool to room temperature after 36 hours to obtain pure colorless block crystals, and determine its molecular structure to be Gd by single crystal X-ray diffractometer. 16 (μ4-F)6(μ3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4; washed three times with acetonitrile and dried, yield 46%.
[0063] The reaction system of the present invention allows the fluorine source that is not easily soluble in organic solvents to be slowly released under high pressure conditions, and the binuclear rare earth precursor prevents the rare earth ions from being directly exposed to the organic solvent. The two prevent the rare earth fluoride precipitation from being generated during the reaction. In addition, by regulating the ratio of the reactant and the deprotonation agent triethylamine, a complete reaction and pure phase gadolinium-based nano-fluorine cluster crystals are obtained. The periphery of the structure is completely wrapped by trimethylacetate and is solvent-free, so it has good thermal stability and corrosion resistance.
[0064] According to the formula -ΔS M=nRln(2s+1), it can be seen that the magnetic entropy change value is determined by the number of nuclei and spin values of the rare earth gadolinium ions. The radius of the fluorine ion is smaller than that of the hydroxide. The gadolinium clusters bridged by hydroxyl groups are usually antiferromagnetic exchange interactions, while the gadolinium clusters bridged by fluorine groups are theoretically ferromagnetic exchange interactions. The ferromagnetic exchange interaction can make its spin value s larger and closer to the ideal value 7 / 2. The magnetic exchange of this material is mainly determined by two fluorine bridging modes μ4-F and μ3-F. When the Gd-F-Gd bond angle is an acute angle, it is an antiferromagnetic exchange interaction such as the μ4-F bridging mode. Therefore, combined with the magnetic characterization results, this material has a weak antiferromagnetic exchange interaction. In addition, since the number of rare earth gadolinium ions n in the structure is 16, the total maximum magnetic entropy change (44.6 J·kg -1 K -1 ) is relatively large, showing excellent magnetic refrigeration performance, and is a good magnetic working fluid material.
Claims
1. A gadolinium-based nanofluorine cluster for magnetic refrigeration, characterized in that: The molecular formula of the structure is Gd 16 ( µ 4-F)6( µ 3-F) 12 [(CH3)3CCOO] 18 [N(CH2CH2O)3]4, µ 4-F and µ 3-F is the bridging mode of fluoride ion, (CH3)3CCOOH is trimethylacetic acid, N(CH2CH2OH)3 is triethanolamine, and the gadolinium-based fluoride bridging cluster is a zero-dimensional nano-sized material.
2. The gadolinium-based nanofluorine cluster for magnetic refrigeration according to claim 1, characterized in that: The application temperature of gadolinium-based fluorine-bridged cluster magnetic refrigeration materials is 0.3K~40K.
3. The gadolinium-based nanofluorine cluster for magnetic refrigeration according to claim 1, characterized in that: The magnetic field applied during the magnetization stage is 0.5T~7T.
4. A method for preparing the gadolinium-based nanofluorine clusters for magnetic refrigeration according to claim 1, characterized in that: The following steps are involved: S1, dissolving and dispersing trimethyl gadolinium acetate, triethanolamine and triethylamine in an organic solvent to obtain a solution A; S2, dispersing the fluorine source in ethanol to obtain solution B, mixing solution A and solution B evenly and then performing a solvothermal reaction, and obtaining a colorless and transparent gadolinium-based fluorine-bridged cluster magnetic refrigeration crystal material by programmed cooling; The fluoride source is one of triethylamine trihydrofluoride, ammonium fluoride, tetramethylammonium fluoride tetrahydrate or sodium fluoride.
5. The method for preparing gadolinium-based nano-fluorine clusters for magnetic refrigeration according to claim 4, characterized in that: The organic solvent is one or a mixture of N,N-dimethylformamide, acetonitrile, anhydrous methanol or ethanol.
6. The method for preparing gadolinium-based nano-fluorine clusters for magnetic refrigeration according to claim 4, characterized in that: The solvent thermal reaction temperature is 120-160°C, the reaction time is 24-72 hours, and the programmed cooling rate is 3-10°C per hour.
7. The method for preparing gadolinium-based nano-fluorine clusters for magnetic refrigeration according to claim 4, characterized in that: The molar ratio of gadolinium trimethylacetate, triethanolamine, triethylamine and fluorine source is 1:0.1~3:0.1~3:0.5~3.
Citation Information
Patent Citations
Rare earth RE2ZnMnO6 oxide magnetic refrigeration material and preparation method thereof
CN111403137A
Method for preparing high-temperature superconducting gadolinium-barium-copper-oxygen thin film by utilizing chemical solution method
CN102603283A
Rare earth-doped alkaline earth metal fluoride nano material, and preparation method and application thereof
CN103224787A
Magnetic refrigeration material containing rare earth hydroxide and preparation method thereof
CN104559944A
Fluorine-bridged rare earth molecular cluster magnetic refrigeration material and preparation method thereof
CN111292909A