A highly corrosion-resistant economical oil well pipe steel and its preparation method

By adopting specific composition and process processing in oil well pipe steel, a mixed structure of ferrite + austenite + martensite is formed, which solves the problems of high cost and insufficient corrosion resistance caused by high Cr content, and achieves low Oil well pipe steel with high strength and excellent corrosion resistance under Cr content is suitable for oil and gas mining in high harsh environments.

CN116145051BActive Publication Date: 2024-11-12CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211593652.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-12
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

The existing oil well pipe steel alloy content is high, resulting in high cost and complex process, which cannot meet the needs of mass production and practical applications, especially in environments containing H2S and CO2. The corrosion resistance performance is insufficient.

Method used

High corrosion-resistant economical oil well pipe steel is used, and the composition includes C: ≤0.03%, Cr: 17.3%~18.4%, Mo: 0.5%~2.0%, Ni: 1.0%~2.8%, Mn: 1.0%~3.5%, Si: 0.1% to 0.5%, N: 0.1% to 0.25%, P: ≤0.03%, S: ≤0.01%, through the mixed structure of ferrite + austenite + martensite, combined with controlled rolling and cooling Thermal deformation process controls the hot rolling and cooling process parameters to obtain excellent corrosion resistance and strength.

Benefits of technology

It achieves high strength and excellent corrosion resistance at low Cr content, significantly improves the resistance to H2S stress corrosion, and is lower than that of traditional high Cr content stainless steel, and is suitable for oil and gas mining in high harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116145051B_ABST
    Figure CN116145051B_ABST
Patent Text Reader

Abstract

The invention discloses a highly corrosion-resistant economical oil well pipe steel and a preparation method thereof, which belongs to the technical field of corrosion-resistant steel and solves the problem of high alloy element content and high cost of oil well pipe steel in the prior art. The components of the highly corrosion-resistant economical oil well pipe steel include, by mass percentage: C: ≤0.03%, Cr: 17.3% to 18.4%, Mo: 0.5% to 2.0%, Ni: 1.0% to 2.8%, Mn: 1.0% to 3.5%, Si: 0.1% to 0.5%, N: 0.1% to 0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities. The oil well pipe steel of the invention has high strength, good plasticity and toughness, and excellent corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of corrosion-resistant steel, and in particular to a highly corrosion-resistant economical oil well pipe steel and a preparation method thereof. Background Art

[0002] Oil well pipes are important consumables in the process of oil and natural gas exploration and development, accounting for about 40% of the total steel used in the oil and gas industry, and are an important component of oil and natural gas extraction equipment. As an important petroleum equipment material, oil well pipes account for an average of 20% to 30% of the entire well construction cost. Therefore, whether the entire petroleum project can proceed smoothly is inseparable from the quality of oil well pipes. The oil well pipe is placed in the casing and is used to collect oil and gas. Due to the flow of corrosive liquids in the oil well pipe, various anti-corrosion products must be selected according to the corrosion conditions. In China, Sichuan gas fields contain H2S, and some oil and gas wells in Sichuan, North China and western oil and gas fields contain CO2 and H2S, CO2, C1 - Coexistence. Under such oil production conditions, higher requirements are also placed on the corrosion resistance of oil well pipes. At present, the material for oil well pipes that resist CO2 corrosion is mainly 13Cr martensitic stainless steel, but martensitic steel cannot be used in environments containing H2S. Although the use of 22Cr (or 25Cr, 27Cr, the higher the Cr content, the better the corrosion resistance) duplex stainless steel with a higher alloy content can meet the use requirements of oil well pipes, the material cost is high and is not suitable for large-scale industrial applications in oil and gas production scenarios. In view of the actual situation of China's oil and gas production and the limitations of mineral resources, it is imperative to develop economical and highly corrosion-resistant oil well pipe materials.

[0003] At present, there are many patents at home and abroad on the varieties and corresponding process flows of oil well pipe steel with good comprehensive performance, but most of them have problems such as high cost or complex process and cannot meet the needs of mass production and practical application. Summary of the invention

[0004] In view of the above situation, the present invention aims to provide a highly corrosion-resistant and economical oil well pipe steel and a preparation method thereof, so as to solve the problem that the existing oil well pipe steel has high alloy element content and high cost.

[0005] The purpose of the present invention is mainly achieved through the following technical solutions:

[0006] On the one hand, the present invention provides a highly corrosion-resistant economical oil well pipe steel. The components of the highly corrosion-resistant economical oil well pipe steel include, by mass percentage, C: ≤0.03%, Cr: 17.3%-18.4%, Mo: 0.5%-2.0%, Ni: 1.0%-2.8%, Mn: 1.0%-3.5%, Si: 0.1%-0.5%, N: 0.1%-0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

[0007] In a possible design, the composition of the highly corrosion-resistant economical oil well pipe steel is Cr+3.3Mo+16N≥26.

[0008] In a possible design, the composition of the highly corrosion-resistant economical oil well pipe steel is 60Ni+17Mn-12Mo-800N≤0.

[0009] In a possible design, the components of the highly corrosion-resistant economical oil well pipe steel may be, by mass percentage, C: 0.01% to 0.03%, Cr: 17.4% to 18.4%, Mo: 1.0% to 2.0%, Ni: 1.0% to 2.7%, Mn: 1.4% to 3.2%, Si: 0.1% to 0.5%, N: 0.13% to 0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

[0010] In a possible design, the microstructure of the highly corrosion-resistant economical oil well pipe steel is a mixed structure of ferrite+austenite+martensite.

[0011] In a possible design, in the microstructure of the highly corrosion-resistant economical oil well pipe steel, the volume percentage of austenite is 20% to 40%, and the volume percentage of martensite is 10% to 40%.

[0012] In a possible design, in the microstructure of the highly corrosion resistant economical oil well pipe steel, the austenite grain size is less than 3 μm.

[0013] On the other hand, the present invention also provides a method for preparing highly corrosion-resistant economical oil well pipe steel, which is used to prepare the highly corrosion-resistant economical oil well pipe steel, comprising:

[0014] Step 1: Melting metal raw materials into molten steel;

[0015] Step 2: smelting the molten steel into continuous casting billets or ingots by continuous casting or mold casting;

[0016] Step 3: Forging the continuous casting billet or ingot into a forging billet;

[0017] Step 4: Roll the forged billet into a tube billet, and obtain highly corrosion-resistant and economical oil well pipe steel by controlling hot rolling and cooling process parameters.

[0018] In a possible design, in step 3, the forging temperature is 1150-1250°C.

[0019] In a possible design, in step 4, controlling the hot rolling and cooling process parameters includes: controlling the starting rolling temperature to be above 1050°C, the final rolling temperature to be above 950°C, the deformation in the first rolling pass to be no more than 30%, and the deformation in the final rolling pass to be no more than 50%.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] a) The highly corrosion-resistant and economical oil well pipe steel of the present invention accurately controls the mass percentage of Cr, Ni, Mn, Mo, and N elements in the steel, and combined with the hot deformation process of controlled rolling and controlled cooling, can obtain a mixed structure of ferrite + austenite + martensite, which greatly improves the corrosion resistance and strength of the oil well pipe steel. Since the 17Cr material of the present invention has ultrafine martensite, the tensile strength of the material is better than that of duplex stainless steel with a higher Cr content, and high strength is achieved with a lower Cr content. Compared with the martensitic stainless steel of the prior art, the stainless steel of the present invention introduces ferrite and austenite to obtain better intergranular corrosion resistance and H2S stress corrosion resistance. The austenite content in the stainless steel of the present invention is much higher than that of martensitic stainless steel. It is difficult to obtain an austenite content greater than 20% in martensitic stainless steel, so the material of the present invention has better hydrogen embrittlement resistance.

[0022] b) The steel of the present invention not only ensures high strength, good plasticity and toughness, and excellent corrosion resistance, but also ensures that the yield strength of the steel of the present invention is greater than 600MPa (e.g. 601-648MPa), the tensile strength is greater than 910MPa (e.g. 911-1010MPa), and the elongation is greater than 22% (e.g. 23%-24%). (180℃) CO2 corrosion rate 0.028g / m 2 h or less (e.g. 0.0203 to 0.0275 g / m 2 h); (200℃) CO2 corrosion rate 0.1g / m 2 h or less (e.g. 0.078 to 0.099 g / m 2 h); pitting corrosion rate 2.5g / m 2 h or less (e.g. 1.693 to 2.433 g / m 2 h); crevice corrosion rate 5.9g / m 2 h or less (e.g. 3.303 to 5.852 g / m 2 h); H2S stress corrosion test was passed.

[0023] c) The steel of the present invention has good toughness and excellent corrosion resistance, and has both the high strength of super martensitic stainless steel oil well pipe materials and the stress corrosion resistance, intergranular corrosion resistance and small amount of H2S stress corrosion resistance of duplex stainless steel. Since the Cr and Ni content of the steel of the present invention is low, the raw material cost is equivalent to or even slightly lower than that of the super 13Cr martensitic stainless steel in the prior art, and the hot working performance is good, so the steel of the present invention has low comprehensive cost, is economical and practical.

[0024] Other features and advantages of the present invention will be described in the following description, and part of them will become obvious from the description, or will be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the written description, claims, and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0026] Figure 1 This is a microstructure diagram of the steel after hot rolling according to Example 1 of the present invention;

[0027] Figure 2 For the present invention Figure 1 Transmission electron microscope image at M in the figure;

[0028] Figure 3 The microstructure diagram of the steel of Example 2 of the present invention;

[0029] Figure 4 The microstructure diagram of the steel of Example 3 of the present invention;

[0030] Figure 5 The microstructure diagram of the steel of Example 4 of the present invention;

[0031] Figure 6 This is a photo of the hot-rolled plate of Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used to illustrate the principles of the present invention together with the embodiments of the present invention.

[0033] The invention provides a highly corrosion-resistant economical oil well pipe steel. The components of the highly corrosion-resistant economical oil well pipe steel include, by mass percentage, C: ≤0.03%, Cr: 17.3%-18.4%, Mo: 0.5%-2.0%, Ni: 1.0%-2.8%, Mn: 1.0%-3.5%, Si: 0.1%-0.5%, N: 0.1%-0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

[0034] Specifically, Cr+3.3Mo+16N (i.e., PREN) ≥ 26, and 60Ni+17Mn-12Mo-800N ≤ 0; wherein Cr, Mo, N, Ni, and Mn refer to the mass percentage of these elements × 100. For example, the mass percentage of the Cr element is 18.4%, and the Cr here is 18.4.

[0035] The following is a detailed description of the effects and dosage of the components in the present invention:

[0036] C: Although the addition of carbon can significantly improve the hardness and strength of steel, due to the high diffusion capacity of carbon, it is easy to combine with Cr to form M 23 C6 type carbide, this type of carbide is mainly precipitated quickly (≤0.5 hours) in the temperature range of 700-900°C, or precipitated when kept at 550-700°C for a long time. The precipitation of carbides causes local Cr deficiency, increases the intergranular corrosion sensitivity of the material, and deteriorates the corrosion resistance. Therefore, in the present invention, the comprehensive effect of strength and corrosion resistance is comprehensively considered, and its content is controlled to be ≤0.03%.

[0037] Cr: The main element to ensure the corrosion resistance of stainless steel. It is also a ferrite-forming element. Improper control of Cr content will increase the ferrite content in the organization and reduce the strength. Considering comprehensive considerations, its content is controlled at 17.3% to 18.4%.

[0038] Ni: It is an element that strongly forms and stabilizes austenite and expands the austenite phase region. Ni is an element that improves the toughness and corrosion resistance of stainless steel in reducing media. Ni is also an important element that improves the resistance of austenite phase to transgranular stress corrosion in various media. At the same time, compared with Mn element, Ni element can reduce the cold working hardening tendency of austenite phase. Considering cost control, the present invention controls its content within 1.0% to 2.8%.

[0039] Mn: It can improve the solubility of N in steel and inhibit the precipitation of harmful phase chromium nitride, but Mn reduces the toughness of stainless steel. Compared with Ni, Mn is an economical austenite-forming element. Mn has different hardening effects on the austenite phase of stainless steel and the overall material. Therefore, the present invention controls its content within 1.0% to 3.5%.

[0040] Mo: In addition to improving the corrosion resistance of stainless steel in oxidizing media, it also has a good effect on improving the corrosion resistance of stainless steel in reducing media. At the same time, in order to ensure pitting resistance, alloy elements such as Cr and Mo that increase the PREN value should not be too low. At the same time, alloy cost control and phase balance must also be considered. Comprehensively considered, its content is controlled to 0.5% to 2.0%.

[0041] Si: Si is added as a deoxidizer during the smelting process to achieve a deoxidation effect. Too much addition will deteriorate the intergranular corrosion resistance of the material. The present invention controls its content to 0.1% to 0.5%.

[0042] N: Like Ni, it is an element that strongly forms and stabilizes austenite and expands the austenite phase. N can also significantly improve the pitting corrosion resistance of the austenite phase in stainless steel, thereby improving the overall pitting corrosion resistance of stainless steel. In some media, N has a good effect on the stress resistance of stainless steel, and there is an optimal value. Further increasing the N content will reduce its stress corrosion resistance. N is also a relatively economical alloying element, but N reduces the hot working performance of stainless steel. Therefore, the present invention controls its content to 0.1% to 0.25%.

[0043] S: It will significantly reduce the hot working performance of steel and easily react with Mn to form MnS inclusions, which will reduce the material's resistance to pitting corrosion and crevice corrosion. Therefore, its content is controlled to ≤ 0.01%.

[0044] P: It is a harmful impurity element that will not only deteriorate the plasticity of the material, but also reduce the corrosion resistance of the material. Therefore, its content is controlled to be ≤0.03%.

[0045] Specifically, the present invention comprehensively considers three aspects: guarantee of corrosion resistance, raw material cost caused by alloy element matching, precipitation of harmful phases caused by alloy element matching, and cost change caused by hot working yield. In addition to controlling the content of individual elements of main alloying elements Cr, Ni, Mn, and N in steel, in order to ensure corrosion resistance, Cr+3.3Mo+16N≥26 is controlled. In order to make the maximum precipitation temperature of harmful phases lower than 750°C and ensure that the material has good hot working performance, and considering that the ratio of the three phases can be controlled during hot working between 900 and 1180°C, it is necessary to control the content of Ni, Mn, Mo, and N elements to meet the following conditions: 60Ni+17Mn-12Mo-800N≤0.

[0046] In order to further improve the comprehensive performance of the above-mentioned highly corrosion-resistant economical oil well pipe steel, the composition of the above-mentioned highly corrosion-resistant economical oil well pipe steel can be calculated by mass percentage as follows: C: 0.01% to 0.03%, Cr: 17.4% to 18.4%, Mo: 1.0% to 2.0%, Ni: 1.0% to 2.7%, Mn: 1.4% to 3.2%, Si: 0.1% to 0.5%, N: 0.13% to 0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities. Among them, Cr+3.3Mo+16N (i.e., PREN) is 26.1 to 27.8, and 60Ni+17Mn-12Mo-800N≤-0.42.

[0047] Specifically, the microstructure of the highly corrosion-resistant economical oil well pipe steel is a mixed structure of ferrite + austenite + martensite, wherein the volume percentage of austenite is 20% to 40% (e.g., 20% to 35%), and the volume percentage of martensite is 10% to 40% (e.g., 30% to 40%), and the martensite is dispersed in the austenite in the form of ultrafine sheets, alternately stacked with the austenite, and divided from each other, so that the austenite has a smaller grain size (e.g., the austenite grain size is <3 μm), and the thickness of the martensite sheet is less than 100 nm.

[0048] Compared with the prior art, the highly corrosion-resistant economical oil well pipe steel of the present invention is a three-phase structure. The steel of the present invention has the characteristics of low Cr and low alloy element content to obtain higher strength. It can also have the characteristics of high strength, resistance to intergranular corrosion, stress corrosion, high toughness and good welding performance, and has excellent comprehensive performance. At the same time, the composite structure of martensite and austenite can increase the interface density in the organization, thereby obtaining high-strength mechanical properties that are superior to traditional duplex stainless steel. Its balanced phase ratio in the conventional hot working temperature range (900-1180°C) brings excellent hot working performance. The multi-phase composite organizational form after hot working has better corrosion resistance than single-phase martensitic stainless steel while ensuring certain cold working performance.

[0049] The present invention also provides a method for preparing the above-mentioned highly corrosion-resistant economical oil well pipe steel, comprising:

[0050] Step 1: Melting metal raw materials into molten steel;

[0051] Step 2: smelting the molten steel into continuous casting billets or ingots by continuous casting or mold casting;

[0052] Step 3: heating the continuous casting billet or ingot at 1150-1250° C., forging and opening the billet to form a forging billet;

[0053] Step 4: Heat the forged billet at 1050-1250°C, roll it into a tube billet, and obtain highly corrosion-resistant economical oil well pipe steel by controlling the hot rolling and cooling process parameters. The three-phase structure content of the highly corrosion-resistant economical oil well pipe steel is: 10%-40% martensite content, 20%-40% austenite content, and the rest is ferrite.

[0054] Specifically, in the above steps 1 and 2, a converter or electric furnace is used for smelting, LF refining and casting into ingots.

[0055] Specifically, in the above step 3, the forging temperature is 1150-1250°C. This is because the material of the present invention is a two-phase ferrite + austenite when it is higher than 800°C. The ratio of the two phases changes with the heating temperature. The higher the heating temperature, the more ferrite content, and the corresponding austenite content decreases. Selecting this temperature range for heating ensures the full dissolution of harmful precipitated phases, and also makes the ferrite phase content in the material greater than 70%, so that the steel is forged in a single-phase region with better thermoplasticity, avoiding the difference in the thermal deformation capacity of the two phases of ferrite and austenite, which leads to the uncoordinated deformation of the two phases in the forging process and causes forging cracking.

[0056] Specifically, in the above step 4, the tube is hot-rolled and then water-cooled to room temperature to avoid the precipitation of harmful phases.

[0057] Specifically, in the above step 4, since the oil well pipe steel of the present invention has an excellent hot working window, controlling the hot rolling and cooling process parameters includes: controlling the starting rolling temperature to be above 1050° C. (e.g., 1050-1200° C.), the final rolling temperature to be above 950° C. (e.g., 950-1050° C.), the deformation amount of the first rolling pass to be no more than 30%, and the deformation amount of the final rolling pass to be no more than 50%.

[0058] Compared with the prior art, the highly corrosion-resistant and economical oil well pipe steel of the present invention accurately controls the mass percentage of Cr, Ni, Mn, Mo, and N elements in the steel, and combined with the hot deformation process of controlled rolling and controlled cooling, can obtain a mixed structure of ferrite + austenite + martensite, which greatly improves the corrosion resistance and toughness of the oil well pipe steel. In stainless steel, the increase of Cr content can improve the strength of the material, but because the 17Cr material of the present invention has ultrafine martensite, the tensile strength of the material is better than that of duplex stainless steel with a higher Cr content. Compared with the duplex stainless steel of the prior art, the 17Cr three-phase structure stainless steel of the present invention controls the content combination of Cr, Ni, Mn, Mo, and N, and obtains a three-phase structure with adjustable martensite content after hot rolling, so as to achieve high strength with a lower Cr content. Compared with the martensitic stainless steel of the prior art, the stainless steel of the present invention introduces ferrite and austenite to obtain better intergranular corrosion resistance and H2S stress corrosion resistance. The austenite content in the stainless steel of the present invention is much higher than that in martensitic stainless steel. It is difficult to obtain an austenite content greater than 20% in martensitic stainless steel. Therefore, the material of the present invention has better hydrogen embrittlement resistance.

[0059] The steel of the present invention not only ensures high strength, good plasticity and toughness, and excellent corrosion resistance, but also ensures that the yield strength of the steel of the present invention is greater than 600MPa (e.g. 601-648MPa), the tensile strength is greater than 910MPa (e.g. 911-1010MPa), and the elongation is greater than 22% (e.g. 23%-24%). (180℃) CO2 corrosion rate 0.028g / m 2h or less (e.g. 0.0203 to 0.0275 g / m 2 h); (200℃) CO2 corrosion rate 0.1g / m 2 h or less (e.g. 0.078 to 0.099 g / m 2 h); pitting corrosion rate 2.5g / m 2 h or less (e.g. 1.693 to 2.433 g / m 2 h); crevice corrosion rate 5.9g / m 2 h or less (e.g. 3.303 to 5.852 g / m 2 h); H2S stress corrosion test was passed.

[0060] The steel of the present invention has good toughness and excellent corrosion resistance, and has both the high strength of super martensitic stainless steel oil well pipe materials and the stress corrosion resistance, intergranular corrosion resistance and small amount of H2S stress corrosion resistance of duplex stainless steel. Since the Cr and Ni content of the steel of the present invention is low, the raw material cost is equivalent to or even slightly lower than that of the super 13Cr martensitic stainless steel in the prior art, and the hot working performance is good, so the steel of the present invention has low comprehensive cost, is economical and practical.

[0061] Examples 1-4

[0062] The advantages of precise control of the composition and process parameters of the steel of the present invention are demonstrated below with specific examples and comparative examples. 13Cr is selected as a comparison object for corrosion performance.

[0063] Examples 1-4 of the present invention provide a highly corrosion-resistant economical oil well pipe steel and a preparation method thereof. The chemical compositions of the steels of Examples 1-4 are shown in Table 1.

[0064] The preparation method of Example 1 comprises:

[0065] Step 1: Melting metal raw materials into molten steel; using a die casting method to smelt the molten steel into steel ingots to obtain ingots;

[0066] Step 2: After heating the ingot to 1150°C and keeping the temperature for 2 hours, forging and opening the ingot to form a forging ingot;

[0067] Step 3: Keep the forging billet at 1050°C for 2h and roll it into a tube billet. By controlling the hot rolling and cooling process parameters (the deformation amount of the first pass is 25%, the deformation amount of the final rolling pass is 48%, the final rolling plate thickness is controlled at about 3.5mm, and water cooling), the final rolling temperature is controlled at 960°C to adjust the three-phase structure content, the ferrite content is 40%, the martensite content is 40%, and the austenite content is 20%.

[0068] The preparation method of Example 2 comprises:

[0069] Step 1: Melting metal raw materials into molten steel; using a die casting method to smelt the molten steel into steel ingots to obtain ingots;

[0070] Step 2: After heating the ingot to 1180°C and keeping the temperature for 1.5 hours, forging and opening the ingot to make a forging ingot;

[0071] Step 3: Keep the forging billet at 1150°C for 2h and roll it into a tube billet. By controlling the hot rolling and cooling process parameters (the deformation amount of the first pass is 28%, the deformation amount of the final rolling pass is 45%, the final rolling plate thickness is controlled at about 3.5mm, and water cooling), and by controlling the final rolling temperature at 1000°C, the three-phase structure content is adjusted to 45% ferrite, 30% martensite, and 25% austenite.

[0072] The preparation method of Example 3 comprises:

[0073] Step 1: Melting metal raw materials into molten steel; using a die casting method to smelt the molten steel into steel ingots to obtain ingots;

[0074] Step 2: After heating the ingot to 1200°C and keeping the temperature for 1 hour, forging and opening the ingot to make a forging ingot;

[0075] Step 3: The forged billet is kept at 1200℃ for 2h and rolled into a tube billet. By controlling the hot rolling and cooling process parameters (the deformation of the first pass is 23%, the deformation of the final rolling pass is 46%, the final rolling thickness is controlled at about 3.5mm, and water cooling), the final rolling temperature is controlled at 1050℃ (the three-phase structure content is adjusted, the ferrite content is 40%, the martensite content is 30%, and the austenite content is 30%).

[0076] The preparation method of Example 4 comprises:

[0077] Step 1: Melting the metal raw materials into molten steel; using a die casting method to smelt the molten steel into ingots to obtain billets;

[0078] Step 2: After heating the ingot to 1250°C and keeping it for 1 hour, forging and blanking are performed to form a forging billet;

[0079] Step 3: Keep the forging billet at 1200℃ for 2h, roll it into a tube billet, and control the hot rolling and cooling process parameters (deformation of the first pass is 26%, deformation of the final rolling pass is 45%, the final rolling plate thickness is controlled at about 3.5mm, water cooling), and adjust the three-phase structure content by controlling the final rolling temperature at 1050℃, with a ferrite content of 35%, a martensite content of 30%, and an austenite content of 35%.

[0080] The specific process parameters of Examples 1-4 are shown in Table 2, and the mechanical properties of Examples 1-4 are shown in Table 3. Figure 1 is a microstructure diagram of the steel of Example 1 of the present invention, Figure 2 The present invention Figure 1The transmission electron microscope image at M in the figure, in which the upper left corner is the diffraction spot of the martensite and austenite matrix at A, which can prove the crystal structure of the black martensite sheet and the thickness of the martensite sheet is less than 100nm.

[0081] Figure 3-Figure 5 The microstructure diagrams of the steels of Examples 2-4 of the present invention are shown in Table 4 below. The microstructure of the highly corrosion-resistant economical oil well pipe steel of the present invention is a mixed structure of ferrite + austenite + martensite, wherein the volume percentage of austenite is 20% to 40% (e.g., 20% to 35%), and the volume percentage of martensite is 10% to 40% (e.g., 30% to 40%), and the martensite is dispersed in the austenite in the form of ultrafine sheets, alternately stacked with the austenite, and divided from each other, so that the austenite has a smaller grain size (e.g., the austenite grain size is <3 μm), and the thickness of the martensite sheet is less than 100 nm.

[0082] Table 1 Chemical composition of Examples 1-4 (wt%)

[0083]

[0084] Table 2 Specific process parameters of Examples 1-4

[0085] serial number Forging temperature, ℃ Hot rolling temperature (start rolling, final rolling), ℃ Example 1 1150 1050、950 Example 2 1180 1150、1000 Example 3 1200 1200、1050 Example 4 1250 1200、1050

[0086] Table 3 Mechanical properties of Examples 1-4

[0087]

[0088] Table 4 Microstructure of steel of Examples 1-4

[0089]

[0090] In order to illustrate the corrosion resistance of the steel of the present invention, the corrosion resistance of the steel of Examples 1-4 was measured under 5 different conditions and compared with 13Cr under the same test conditions. This experiment was used to evaluate the corrosion resistance of the steel of the present invention in different corrosive environments. The results of the corrosion test are shown in Table 5, and the corresponding test conditions are as follows:

[0091] (180℃ or 200℃) The corrosion conditions of CO2 corrosion rate are as follows:

[0092] 1. Medium (formation water) mg / L: CO3 2- / 0,HCO3 - / 189,OH - / 0,Cl - / 128000,SO4 2- / 430,Ca 2+ / 8310,Mg2+ / 561,K + / 6620,Na + / 76500);

[0093] 2. CO2 partial pressure: 4.48MPa, total test pressure: 10MPa;

[0094] 3. Test temperature: 180℃ or 200℃;

[0095] 4. Test time: 720 hours.

[0096] The corrosion conditions for pitting corrosion rate are as follows:

[0097] 1. Test temperature: 22±2℃;

[0098] 2. Medium: 100g reagent grade ferric chloride FeCl3·6H2O dissolved in 900mL IV reagent grade water (mass ratio about 6%);

[0099] 3. Test time: 72 hours;

[0100] 4. Sample size: 50×25×3mm, polished to 2000# sandpaper.

[0101] The corrosion conditions for crevice corrosion rate are as follows:

[0102] 1. The test temperature is 22±2℃;

[0103] 2. Dissolve 100g reagent grade ferric chloride FeCl3·6H2O in 900mL IV reagent grade water (mass ratio about 6%);

[0104] 3. Test time: 72 hours;

[0105] 4. Sample size: 50×25×3mm, polished to 2000# sandpaper.

[0106] The corrosion conditions of H2S stress corrosion test are as follows:

[0107] 1. The test temperature is 22±2℃;

[0108] 2. 50 g NaCl, 25 g [23.8 mL] CH3COOH, and 4.1 g CH3COONa were dissolved in 921 mL IV reagent grade water (about 5 wt% sodium chloride, 2.5 wt% glacial acetic acid, and 0.41 wt% sodium acetate by mass ratio);

[0109] 3. Test time: 720 hours;

[0110] 4. Sample size: 50×5×2mm, polished to 2000# sandpaper;

[0111] 5. Four-point bending test, loading force is 80% yield stress.

[0112] From Table 5, it can be seen that the (180°C) CO2 corrosion rate of the highly corrosion-resistant economical oil well pipe steel of Examples 1-4 is 0.028 g / m 2 h or less (e.g. 0.0203 to 0.0275 g / m 2 h); (200℃) CO2 corrosion rate 0.1g / m 2 h or less (e.g. 0.078 to 0.099 g / m 2 h); pitting corrosion rate 2.5g / m 2 h or less (e.g. 1.693 to 2.433 g / m 2 h); crevice corrosion rate 5.9g / m 2 h or less (e.g. 3.303 to 5.852 g / m 2 h); H2S stress corrosion test was passed. The corrosion resistance of Examples 1-4 of the present invention is better than that of 13Cr, especially the CO2 corrosion resistance at 200°C. The present invention is far better than super 13Cr and can be used in more demanding environments, that is, in environments with greater well depths. Figure 5 Shown is a graph showing the results of the H2S stress corrosion test of Example 1.

[0113] Table 5 Corrosion test data

[0114]

[0115]

[0116] In order to illustrate the hot working performance of the steel of the present invention, the edge quality of the steel plates after hot rolling in Examples 1-4 is statistically analyzed, with Example 1 being taken as an example. Figure 6 The hot-rolled plate of Example 1 is shown in the figure. It can be seen that there is no cracking at the edge. The yield rate of the steel of the example of the present invention in the actual production process reaches more than 90%.

[0117] The inventors have conducted a lot of in-depth research in the research, and now some of the solutions with poor effects are listed as comparative examples as follows:

[0118] Comparative Example 1

[0119] The present comparative example provides a corrosion-resistant oil well pipe steel and a preparation method thereof. The corrosion-resistant oil well pipe steel of the present comparative example is 13Cr and is prepared by the current mature process of 13Cr. The composition of the corrosion-resistant oil well pipe steel of the present comparative example is C: 0.03%, Cr: 13%, Ni: 5%, Mo: 2%, Mn: 0.5%, Si: 0.5%, and the preparation method is as follows: after heating and forging at 1150°C, water cooling, reheating to 860°C for 2h, quenching, and tempering at 620°C for 1h.

[0120] The microstructure of the steel of this comparative example is martensite (93%) + austenite (7%). The mechanical properties are shown in Table 3 above, and the corrosion resistance results are shown in Table 5 above.

[0121] Comparative Example 2

[0122] This comparative example provides a corrosion-resistant oil well pipe steel and a preparation method thereof. The corrosion-resistant oil well pipe steel of this comparative example has the following components: C: 0.03%, Cr: 16%, Mo: 1.21%, N: 0.22%, Mn: 2.11%, and Si: 0.5%. The preparation method is the same as that of Example 1.

[0123] The microstructure of the steel of this comparative example is ferrite (15%) + martensite (65%) + austenite (20%). The mechanical properties are shown in Table 3, and the corrosion resistance results are shown in Table 5.

[0124] Comparative Example 3

[0125] This comparative example provides a corrosion-resistant oil well pipe steel and a preparation method thereof. The corrosion-resistant oil well pipe steel of this comparative example has the following components: C: 0.04%, Cr: 16.5%, Ni: 1.12%, Mo: 1.32%, N: 0.16%, Mn: 2.82%, and Si: 0.5%. The preparation method is the same as that of Example 1.

[0126] The microstructure of the steel of this comparative example is ferrite (20%) + martensite (60%) + austenite (20%). The mechanical properties are shown in Table 3, and the corrosion resistance results are shown in Table 5.

[0127] By comparing the embodiments and comparative examples, it can be seen that the highly corrosion-resistant and economical oil well pipe steel of the present invention accurately controls the mass percentages of Cr, Ni, Mn, Mo, and N elements in the steel, and combines the hot deformation process of controlled rolling and controlled cooling to obtain a mixed structure of ferrite + austenite + martensite, which greatly improves the corrosion resistance and toughness of the oil well pipe steel. The raw material cost is equivalent to or even slightly lower than that of the super 13Cr martensitic stainless steel in the prior art, and the hot working performance is good. The corrosion resistance of the highly corrosion-resistant and economical oil well pipe steel of the present invention is better than that of the super 13Cr martensitic stainless steel. Therefore, the steel of the present invention has low comprehensive cost, is economical, and is practical.

[0128] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A highly corrosion-resistant economical oil well pipe steel, characterized in that: The components of the highly corrosion-resistant economical oil well pipe steel include, by mass percentage, C: ≤0.03%, Cr: 17.3%~18.4%, Mo: 0.5%~2.0%, Ni: 1.0%~2.8%, Mn: 2.01%~3.5%, Si: 0.1%~0.5%, N: 0.17%~0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities; In the composition of the highly corrosion-resistant economical oil well pipe steel, Cr+3.3Mo+16N≥26, 60Ni+17Mn-12Mo-800N≤0; wherein Cr, Mo, N, Ni, and Mn refer to the mass percentage of these elements × 100; The microstructure of the highly corrosion-resistant economical oil well pipe steel is a mixed structure of ferrite + austenite + martensite; the volume percentage of austenite is 20% to 40%, and the volume percentage of martensite is 10% to 40%; Martensite is dispersed in austenite in the form of ultrafine flakes, alternately stacked with austenite, and divided from each other, making the austenite have a smaller grain size. The austenite grain size is less than 3 μm. The preparation method of the highly corrosion-resistant economical oil well pipe steel is as follows: Step 1: Melting metal raw materials into molten steel; Step 2: smelting the molten steel into continuous casting billets or ingots by continuous casting or mold casting; Step 3: Forging the continuous casting billet or ingot into a forging billet; Step 4: Roll the forged billet into a tube billet, and obtain highly corrosion-resistant and economical oil well pipe steel by controlling hot rolling and cooling process parameters.

2. The highly corrosion-resistant economical oil well pipe steel according to claim 1, characterized in that: In the composition of the highly corrosion-resistant economical oil well pipe steel, Cr+3.3Mo+16N is 26.1-27.

8.

3. The highly corrosion-resistant economical oil well pipe steel according to claim 1, characterized in that: Among the components of the highly corrosion-resistant economical oil well pipe steel, 60Ni+17Mn-12Mo-800N≤-0.

42.

4. The highly corrosion-resistant economical oil well pipe steel according to claim 1, characterized in that: The components of the highly corrosion-resistant economical oil well pipe steel are, by mass percentage, C: 0.01%-0.03%, Cr: 17.4%-18.4%, Mo: 1.0%-2.0%, Ni: 1.0%-2.7%, Mn: 2.01%-3.2%, Si: 0.1%-0.5%, N: 0.17%-0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

5. The highly corrosion-resistant economical oil well pipe steel according to claim 1, characterized in that: In the microstructure of the highly corrosion-resistant economical oil well pipe steel, the volume percentage of austenite is 20% to 35%, and the volume percentage of martensite is 30% to 40%.

6. A method for preparing highly corrosion-resistant economical oil well pipe steel, characterized in that: Used to prepare the highly corrosion-resistant economical oil well pipe steel according to any one of claims 1 to 5, comprising: Step 1: Melting metal raw materials into molten steel; Step 2: smelting the molten steel into continuous casting billets or ingots by continuous casting or mold casting; Step 3: Forging the continuous casting billet or ingot into a forging billet; Step 4: Roll the forged billet into a tube billet, and obtain highly corrosion-resistant and economical oil well pipe steel by controlling hot rolling and cooling process parameters.

7. The preparation method according to claim 6, characterized in that: In the step 3, the forging temperature is 1150-1250°C.

8. The preparation method according to any one of claims 6 to 7, characterized in that: In step 4, controlling the hot rolling and cooling process parameters includes: controlling the starting rolling temperature to be above 1050° C., the final rolling temperature to be above 950° C., the deformation of the first rolling pass to be no more than 30%, and the deformation of the final rolling pass to be no more than 50%.