A 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel and its application

By carrying a 3D scaffold carrying oleanolic acid nanoparticles/chitosan composite hydrogel, the problem of bioavailability and pharmacodynamic activity of oleanolic acid in the treatment of oral cancer has been solved, and the treatment of oral squamous cancer has been achieved. Effective inhibition and destruction of tumor tissue.

CN116159064BActive Publication Date: 2024-10-29JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211664561.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-10-29
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

It is difficult to effectively improve the bioavailability and pharmacodynamic activity of oleanolic acid with existing technology, resulting in its poor effect in the treatment of oral cancer.

Method used

A 3D scaffold carrying oleanolic acid nanoparticles/chitosan composite hydrogel is used. Oleanolic acid is wrapped with a polymer to form nanoparticles, mixed with chitosan hydrogel, and implanted into the 3D scaffold for use. Efficiently inhibit tumor cells and destroy tumor tissue.

Benefits of technology

The pharmacodynamic activity of oleanolic acid is significantly improved, and the tumor inhibitory effect is verified in the oral squamous carcinoma nude mouse transplanted tumor model, effectively inhibiting and destroying tumor tissue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116159064B_ABST
    Figure CN116159064B_ABST
Patent Text Reader

Abstract

The present invention provides a 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel and an application thereof. Oleanolic acid is encapsulated by a polymer to form nanoparticles, a drug solution is mixed with a PVA aqueous solution to obtain a mixed solution, and the mixed solution is quickly and fully mixed by a homogenizer. The fully mixed mixed solution is then placed on a magnetic stirrer to collect the nanoparticles, and the nanoparticles are then mixed with the chitosan hydrogel and implanted into the 3D scaffold in a specific ratio. The scaffold is implanted near the tumor tissue and used for the treatment of oral tumor diseases and head and neck tumor diseases. The scaffold can efficiently inhibit tumor cells and effectively destroy tumor tissue.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a pharmaceutical composition, in particular to a 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel and application thereof. Background Art

[0002] Oral squamous cell carcinoma (OC-SCC) is the most common malignancy in the head and neck, and recent trends indicate that the incidence of oropharyngeal squamous cell carcinoma (OP-SCC) has increased dramatically. Seeking prevention and treatment of oral cancer is a long-term strategy to control the development of cancer.

[0003] In China, oleanolic acid has been used as an over-the-counter (OTC) liver-protecting drug for decades. Recently, it has been found to have great application prospects in anti-cancer. Oleanolic acid (OA) is an oleanane-type pentacyclic triterpenoid compound, a natural plant extract, widely distributed in nature in free form or in the form of glycosides combined with sugars. It exists in the leaves of Olea europaea and Ligustrum lucidum fruits of the Oleaceae family; the whole herb of Swertia chuanxiensis and Green Leaf Gallbladder of the Gentianaceae family; the leaves and roots of Celery of the Apiaceae family; the root bark and stem bark of Demu of the Araliaceae family; and the tubers of the large-seeded snow stork, lovely snow stork, and Chinese snow stork (Golden Toad Lotus, Luoguodi) of the Cucurbitaceae family. It has multiple pharmacological effects such as liver protection, anti-inflammatory, antiviral, antioxidant, and immune regulation. OA has low water solubility and poor oral absorption, but in view of its precise pharmacological effects, domestic and foreign scholars have done a lot of research on its modification, using OA as a lead compound to synthesize OA derivatives, and through the study of the derivatives obtained to screen and explore substances with greater biological activity potential. The pentacyclic triterpene skeleton of oleanolic acid is highly rigid, and there is a lack of water-soluble fragments in the structure, which leads to its poor water solubility, and poor water solubility directly affects bioavailability and biological activity.

[0004] Nanomaterials have great potential in the medical field based on their special nano-scale material properties. When the particle diameter is reduced to the nanoscale, it shows a unique large molecular surface area, relatively high surface reactivity, and many surface active centers, and strong adsorption capacity in molecular metabolism. These characteristics are greatly conducive to the transfer of molecules between cells after nanoparticles enter the body, and are easier to penetrate the cell membrane. At the same time, while encapsulating and adsorbing chemical drugs as carrier preparations, it makes it easier to effectively modify the surface of the material, and also provides strong feasibility and operability for the technical level. In the treatment of tumors, nanoparticles have been widely used as drug delivery systems in oral cancer, breast cancer, ovarian cancer, lung cancer, etc., with their unique and good drug solubility, high drug circulation times, and outstanding advantages in efficacy. All these determine that nanomaterials can play a better role in targeted therapy as a carrier system. At the same time, it also increases the targeting components and stimulation reactions, increases the circulation time of drugs in the body, and increases the release capacity of nanomaterials in the molecular mechanism of disease treatment. In the prevention and treatment of oral cancer, most drugs represented by bioactive plant compounds have certain effects in the prevention of oral cancer, although clinical studies have shown that such natural plant compounds generally have low bioavailability in the treatment of the body, and their biosolubility in the body is relatively poor. We hope that nanotechnology can solve this problem, but the fact is that up to now, there is still no better way to truly overcome this problem. Even if the solubility problem is solved, the pharmacodynamic activity of the drug is still not high, and the effect is still not ideal. The root cause is that the carrier or encapsulation technology may limit the pharmacodynamic activity of oleanolic acid itself, and it does not really play its full pharmacodynamic effect.

[0005] There are many types of three-dimensional biological scaffold material immunotherapy platforms, which can be classified according to their composition, preparation method, route of administration or immunomodulatory principle. In terms of composition, they are usually composed of natural ingredients or synthetic polymers (such as collagen, alginate, hyaluronic acid, PEG, PLGA, mesoporous silica, etc.). In terms of preparation methods, three-dimensional macroscopic structures can usually be constructed by simple cross-linking in vitro, rapid sol-gel phase transition in vivo, in situ chemical polymerization assembly or advanced 3D printing and self-assembly technology. With tumor antigens and adjuvants, immunostimulatory or immunosuppressive molecules, and even bioactive immune cells, these three-dimensional scaffolds or hydrogels have become more diversified. They can also be further loaded with other chemotherapeutic drugs and light / acoustic / thermal / magnetic sensitizers to mediate combined immunotherapy. In addition, due to the importance of three-dimensional in vitro models in scientific research, three-dimensional macroscopic scaffolds also have great potential in the development of bionic organoids, and dynamic biological processes and therapeutic processes can be evaluated simultaneously. Currently, four major strategies are being used to study the design routes and applications of existing 3D bioscaffold materials in tumor immunotherapy, including the use of 3D delivery platforms for immune preparations or cell delivery strategies, 3D scaffolds themselves exerting immune regulatory functions, 3D scaffold biomaterials combined with immunotherapy strategies, and 3D scaffolds as engineering immune regulation models for further cancer immunotherapy research and clinical transformation. Summary of the invention

[0006] The purpose of the present invention is to provide a 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel, in which oleanolic acid is encapsulated by a polymer to form nanoparticles, and then the nanoparticles are mixed with chitosan hydrogel and implanted into the 3D scaffold in a specific ratio, which is then implanted near the tumor tissue for the treatment of oral tumor diseases and head and neck tumor diseases, and can efficiently inhibit tumor cells and effectively destroy tumor tissue.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel, the preparation method of which comprises the following steps:

[0009] Weigh 20-50 mg of polyvinyl alcohol (PVA) and dissolve it in 100-500 mL of distilled water to obtain a PVA aqueous solution, then weigh 40-200 mg of a polymer and 15-100 mg of oleanolic acid and dissolve them in 10-100 mL of dichloromethane to obtain a drug solution; after 24 hours, mix the drug solution with the PVA aqueous solution to obtain a mixed solution, and quickly mix it with a homogenizer at a speed of 4000-9000 r / min for 10-25 minutes, then place the mixed mixed solution under magnetic stirring at a speed of 200 r / min for 12-24 hours, then collect nanoparticles, mix the nanoparticles with chitosan hydrogel to obtain a composite hydrogel, mix the nanoparticles with chitosan in a ratio of 1:1-3, and implant the composite hydrogel into a 3D scaffold, wherein the mass ratio of the 3D scaffold to the composite hydrogel is 1-5:1-3.

[0010] As a more optimal technical solution of the present invention: the polymer is one of polylactic acid polyethylene glycol, polylactic acid glycolic acid polyethylene glycol and polylactic acid.

[0011] As a more optimal technical solution of the present invention: weigh 35 mg of PVA and dissolve it in 260 mL of distilled water to obtain a PVA aqueous solution.

[0012] As a more optimal technical solution of the present invention: weigh 100 mg of PLA-PEG copolymer and 45 mg of oleanolic acid and dissolve them in 100 mL of dichloromethane to obtain a drug solution.

[0013] As a more optimal technical solution of the present invention: after 24 hours, the drug solution is mixed with the PVA aqueous solution to obtain a mixed solution, and the mixed solution is quickly and fully mixed with a homogenizer at a speed of 5000 r / min for 25 minutes.

[0014] As a more optimal technical solution of the present invention: the nanoparticles and chitosan are mixed in a ratio of 1:2.

[0015] Another object of the present invention is to provide the 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel for use in preparing drugs for inhibiting and destroying oral squamous cell carcinoma cells.

[0016] The present invention improves the pharmacodynamic activity by using a combination of multiple preparations, and overcomes the problem that oleanolic acid is not effective in treating tumor diseases. The present invention verifies that the oral squamous cell carcinoma nude mouse transplant tumor model has excellent tumor inhibition effect after using a 3D scaffold carrying oleanolic acid to carry a composite hydrogel, effectively inhibiting tumor cells and effectively destroying tumor tissue. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a diagram of the cell status after the oral cancer cells are treated in Example 1 of the present invention.

[0018] Figure 2 This is a diagram of the cell status after the oral cancer cells were treated in Example 2 of the present invention.

[0019] Figure 3 This is a diagram of the cell status after the oral cancer cells were treated in Example 3 of the present invention.

[0020] Figure 4 This is a diagram of the cell status after the oral cancer cells were treated in Example 4 of the present invention.

[0021] Figure 5 This is a diagram of the cell status after the oral cancer cells were treated in Example 5 of the present invention.

[0022] Figure 6 This is a diagram of the cell status after the oral cancer cells were treated in Example 6 of the present invention.

[0023] Figure 7 This is a diagram of the cell status after the oral cancer cells were treated in Comparative Example 1 of the present invention.

[0024] Figure 8 This is a diagram of the cell status after the oral cancer cells were treated in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0025] The present invention is further defined in the following examples. Based on the following description and these examples, those skilled in the art can ascertain the essential characteristics of the present invention and, without departing from the essence and scope of the present invention, can make various changes and modifications to the present invention to adapt it to various uses and conditions.

[0026] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels.

[0027] Embodiment 1:

[0028] Weigh 35 mg of polyvinyl alcohol (PVA) and dissolve it in 260 mL of distilled water to obtain a PVA aqueous solution, then weigh 100 mg of PLGA-PEG copolymer and 45 mg of oleanolic acid and dissolve them in 90 mL of dichloromethane to obtain a drug solution; after 24 hours, mix the drug solution with the PVA aqueous solution to obtain a mixed solution, and quickly mix it with a homogenizer at a speed of 4000 r / min for 25 minutes, then place the mixed solution under magnetic stirring at a speed of 200 r / min for 24 hours, collect nanoparticles, mix the nanoparticles with chitosan hydrogel to obtain a composite hydrogel, mix the nanoparticles with chitosan in a ratio of 1:2, and implant the composite hydrogel into a 3D scaffold, wherein the mass ratio of the scaffold to the composite hydrogel is 1:1.

[0029] Embodiment 2:

[0030] Weigh 50 mg of polyvinyl alcohol (PVA) and dissolve it in 500 mL of distilled water to obtain a PVA aqueous solution, then weigh 200 mg of PLGA-PEG copolymer and 100 mg of oleanolic acid and dissolve them in 100 mL of dichloromethane to obtain a drug solution; after 24 hours, mix the drug solution with the PVA aqueous solution to obtain a mixed solution, and quickly mix it with a homogenizer at a speed of 9000 r / min for 10 minutes, then place the mixed solution under magnetic stirring at a speed of 200 r / min for 12 hours, collect nanoparticles, mix the nanoparticles with chitosan hydrogel to obtain a composite hydrogel, mix the nanoparticles with chitosan in a ratio of 1:1, and implant the composite hydrogel into a 3D scaffold, wherein the mass ratio of the scaffold to the composite hydrogel is 5:1.

[0031] Embodiment 3:

[0032] Weigh 20 mg of polyvinyl alcohol (PVA) and dissolve it in 100 mL of distilled water to obtain a PVA aqueous solution, then weigh 40 mg of PLGA-PEG copolymer and 15 mg of oleanolic acid and dissolve them in 10 mL of dichloromethane to obtain a drug solution; after 24 hours, mix the drug solution with the PVA aqueous solution to obtain a mixed solution, and quickly mix it with a homogenizer at a speed of 6000 r / min for 10 minutes, then place the mixed solution under magnetic stirring at a speed of 200 r / min for 24 hours, collect nanoparticles, mix the nanoparticles with chitosan hydrogel to obtain a composite hydrogel, mix the nanoparticles with chitosan in a ratio of 1:1, and implant the composite hydrogel into a 3D scaffold, wherein the mass ratio of the scaffold to the composite hydrogel is 3:1.

[0033] Embodiment 4:

[0034] Weigh 35 mg of polyvinyl alcohol (PVA) and dissolve it in 260 mL of distilled water to obtain a PVA aqueous solution, then weigh 200 mg of PLGA-PEG copolymer and 45 mg of oleanolic acid and dissolve them in 90 mL of dichloromethane to obtain a drug solution; after 24 hours, mix the drug solution with the PVA aqueous solution to obtain a mixed solution, and quickly mix it with a homogenizer at a speed of 6000 r / min for 20 minutes, then place the mixed solution under magnetic stirring at a speed of 200 r / min for 24 hours, collect nanoparticles, mix the nanoparticles with chitosan hydrogel to obtain a composite hydrogel, mix the nanoparticles with chitosan in a ratio of 1:3, and implant the composite hydrogel into a 3D scaffold, wherein the mass ratio of the scaffold to the composite hydrogel is 1-5:1-3.

[0035] Embodiment 5:

[0036] Weigh 35 mg of polyvinyl alcohol and dissolve it in 260 mL of distilled water to obtain a PVA aqueous solution, then weigh 150 mg of PLGA-PEG copolymer and 45 mg of oleanolic acid and dissolve them in 90 mL of dichloromethane to obtain a drug solution; after 24 hours, mix the drug solution with the PVA aqueous solution to obtain a mixed solution, and quickly mix it with a homogenizer at a speed of 6000 r / min for 25 minutes, then place the mixed solution under magnetic stirring at a speed of 200 r / min for 12-24 hours, collect nanoparticles, mix the nanoparticles with chitosan hydrogel to obtain a composite hydrogel, mix the nanoparticles with chitosan in a ratio of 1:3, and implant the composite hydrogel into a 3D scaffold, wherein the mass ratio of the scaffold to the composite hydrogel is 1:2.

[0037] Embodiment 6:

[0038] Weigh 35 mg of polyvinyl alcohol and dissolve it in 260 mL of distilled water to obtain a PVA aqueous solution, then weigh 45 mg of PLGA-PEG copolymer and 45 mg of oleanolic acid and dissolve them in 90 mL of dichloromethane to obtain a drug solution; after 24 hours, mix the drug solution with the PVA aqueous solution to obtain a mixed solution, and quickly mix it with a homogenizer at a speed of 6000 r / min for 20 minutes, then place the mixed solution under magnetic stirring at a speed of 200 r / min for 24 hours, collect nanoparticles, mix the nanoparticles with chitosan hydrogel to obtain a composite hydrogel, mix the nanoparticles with chitosan in a ratio of 1:3, and implant the composite hydrogel into a 3D scaffold, wherein the mass ratio of the scaffold to the composite hydrogel is 1:2.

[0039] Comparative Example 1

[0040] The difference between this embodiment and embodiment 1 is that chitosan hydrogel is not added.

[0041] Comparative Example 2

[0042] The difference between this embodiment and embodiment 1 is that oleanolic acid is made into nanoparticles and directly mixed with chitosan hydrogel.

[0043] Comparative Example 3

[0044] The difference between this embodiment and embodiment 1 is that 80 mg of PVA was weighed.

[0045] Comparative Example 4

[0046] The difference between this embodiment and embodiment 1 is that 260 mg of polymer and 10 mg of oleanolic acid were weighed.

[0047] Comparative Example 5

[0048] The difference between this example and Example 1 is that 220 mg of the polymer and 10 mg of oleanolic acid were weighed.

[0049] Comparative Example 6

[0050] The difference between this embodiment and embodiment 1 is that the speed of the homogenizer is 3000r / min and the time is 5min.

[0051] Comparative Example 7

[0052] The difference between this embodiment and embodiment 1 is that the speed of the homogenizer is 9500r / min and the time is 25min.

[0053] Comparative Example 8

[0054] The difference between this embodiment and embodiment 1 is that the nanoparticles and chitosan are mixed in a ratio of 7:1, and the composite hydrogel is implanted into the 3D scaffold.

[0055] Comparative Example 9

[0056] The difference between this embodiment and embodiment 1 is that the nanoparticles and chitosan are mixed in a ratio of 10:1, and the composite hydrogel is implanted into the 3D scaffold.

[0057] The anti-tumor effect of the 3D scaffolds prepared in the above examples and comparative examples was tested.

[0058] First, cell culture was performed: oral squamous cell carcinoma cell line SCC-25 was cultured in DMEM / F-12 medium at a certain initial density in a 37°C, 5% CO2 incubator. Logarithmic phase cells were used for the experiment. Oral cancer cell viability determination test steps: Collect logarithmic phase cells: adjust the cell suspension to 2.5×104 cells / ml, use a spray gun to inoculate SCC-15 and SCC-4 cells in 3 96-well plates, and add 200μl to each well. The 96-well plates were placed in a 37°C, 5% CO2 incubator for 24 hours, and the culture solution containing the example was added after the cells adhered to the wall. The final concentration of the example calculated as a drug was 50mmol / L. The 96-well plates were placed in a 37°C, 5% CO2 incubator and continued to be cultured for 24h, 48h, and 72h, respectively. The 96-well culture plates that were cultured for 48h and 72h were changed every 24h and the example was added. After the cells were treated in different embodiments for 24h, 48h, and 72h, 20μl of 5mg / ml MTT solution was added to each well and cultured for 4h at 37°C in the dark. The culture was terminated and the culture medium in the well was carefully aspirated. 150μl of dimethyl sulfoxide (DMSO) was added to each well and the cells were placed on a shaker and shaken at a low speed for 10 minutes to fully dissolve the crystals. The optical density OD value of each well at 490nm was measured by an ELISA instrument.

[0059] The example showed that the SCC-25 cells treated with the drug for 48h and 72h showed an obvious effect of inhibiting cell growth compared with the control group. The inhibitory effect on the growth of oral cancer cells was very significant, and the OD value gradually decreased with the progress of time, approaching zero at 72 hours.

[0060] OD values ​​under the influence of each group of embodiments

[0061] Group 48h 72h Blank Group 0.51 0.62 Example 1 0.16 0.01 Example 2 0.18 0.05 Example 3 0.18 0.09 Example 4 0.18 0.06 Example 5 0.17 0.02 Example 6 0.19 0.07 Comparative Example 1 0.41 0.29 Comparative Example 2 0.46 0.40 Comparative Example 3 0.30 0.26 Comparative Example 4 0.31 0.20 Comparative Example 5 0.29 0.24 Comparative Example 6 0.22 0.19 Comparative Example 7 0.34 0.31 Comparative Example 8 0.22 0.15 Comparative Example 9 0.26 0.13

[0062] Colorimetric determination is based on the principle that mitochondria of living cells reduce tetramethyl azo blue to purple crystals, which indirectly indicates the number of living cells and reflects the cell proliferation to a certain extent, and explores the cell proliferation status and the effect of foreign chemicals on cell proliferation in vitro. Figures 1 to 8 The MTT method of the present invention is shown to detect the proliferation activity of SCC-25 cells treated with different embodiments. The results show that the embodiments have an inhibitory effect on the growth of human oral cancer cells, and the inhibitory effect is method-dependent, that is, in each embodiment, when the cells are treated according to the embodiments of the invention, it is found under microscopic observation that individual SCC-25 cells have a reduced volume and a rounded shape. As time progresses, it can be seen under microscopic observation that SCC-25 cells have a reduced volume and a rounded shape, and some cells fall off from the attached state and are suspended in the culture medium. As the culture time progresses, the number of detached cells gradually increases. This shows that the long-term action of the embodiments can cause cell death, while the comparative examples are the opposite.

[0063] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel, characterized in that: The preparation method comprises the following steps: weighing 20-50 mg of polyvinyl alcohol and dissolving it in 100-500 mL of distilled water to obtain a PVA aqueous solution, then weighing 40-200 mg of a polymer and 15-100 mg of oleanolic acid and dissolving them in 10-100 mL of dichloromethane to obtain a drug solution; after 24 hours, mixing the drug solution with the PVA aqueous solution to obtain a mixed solution, and quickly mixing the mixed solution with a homogenizer at a speed of 4000-9000 r / min for 10-25 minutes, then placing the mixed solution under magnetic stirring at a speed of 200 r / min for 12-24 hours, collecting nanoparticles, mixing the nanoparticles with chitosan hydrogel to obtain a composite hydrogel, mixing the nanoparticles with chitosan at a ratio of 1:1-3, and implanting the composite hydrogel into a 3D scaffold, wherein the mass ratio of the 3D scaffold to the composite hydrogel is 1-5:1-3; The polymer is polylactic acid-glycolic acid polyethylene glycol.

2. The 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel according to claim 1, characterized in that: Weigh 35 mg of PVA and dissolve it in 260 mL of distilled water to obtain a PVA aqueous solution.

3. The 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel according to claim 1, characterized in that: 100 mg of PLA-PEG copolymer and 45 mg of oleanolic acid were weighed and dissolved in 100 mL of dichloromethane to obtain a drug solution.

4. The 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel according to claim 1, characterized in that: The speed of the homogenizer is 5000r / min, and the time is 25min.

5. The 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel according to claim 1, characterized in that: The nanoparticles are mixed with chitosan in a ratio of 1:

2.

6. The 3D scaffold carrying oleanolic acid nanoparticles / chitosan composite hydrogel according to claim 1, characterized in that: Used to prepare drugs for inhibiting and destroying oral squamous cell carcinoma cells.