Liquid rubber and modified carbon black synergistically toughened epoxy resin and preparation method thereof

Through the epoxy resin technology that synergizes the toughening of liquid rubber and modified carbon black, a cross-linking network is formed, which solves the problem of the lack of obvious improvement of toughness and aging resistance after curing of epoxy resin, and achieves significant mechanical properties and high temperature resistance. Improved aging performance.

CN116162328BActive Publication Date: 2024-12-06JIASHAN HENGXING ELECTRIC POWER CONSTR CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211611248.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-12-06
Estimated Expiration
2042-12-14

AI Technical Summary

Technical Problem

The toughness and aging resistance of epoxy resin after curing are not significantly improved, especially under high temperature and ultraviolet rays and other conditions, the mechanical properties of the material are degraded.

Method used

Using liquid rubber and modified carbon black synergistic epoxy resin, a cross-linking network is formed through inorganic and organic modifiers, improving mechanical properties and anti-aging properties, and optimizing through specific preparation steps and additive combinations to reduce modification dosage of the agent.

Benefits of technology

It significantly improves the bending strength, high-temperature aging resistance and brittle cracking after curing of epoxy resin, and is not easy to crack at low temperatures, significantly improving the overall performance of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of epoxy resin toughening. In order to solve the problem that the prior art has no obvious effect on improving the toughness and aging resistance of epoxy resin after curing, a liquid rubber and modified carbon black synergistically toughened epoxy resin is disclosed, comprising the following weight components: 70-100 parts of epoxy resin, 20-30 parts of curing agent, 0.2-1 parts of catalyst, 30-60 parts of liquid rubber, 2-10 parts of modified carbon black, 0.25-1 parts of antioxidant, and 0.25-1 parts of ultraviolet absorber. The present invention has excellent bending strength, high temperature aging resistance, is not easy to crack, has low moisture absorption rate, and is not easy to crack at low temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy resin toughening, and in particular to an epoxy resin toughened synergistically by liquid rubber and modified carbon black and a preparation method thereof. Background Art

[0002] Epoxy resin cured products have good mechanical properties and excellent electrical properties, and are widely used in power systems, rail transit, new energy and other fields. However, epoxy resin has poor toughness. At the same time, during the use of epoxy resin cured products, they are inevitably affected by the synergistic effects of multiple factors such as temperature, humidity, electricity, and light, which lead to the aging of epoxy resin cured products. Under the combined effects of high temperature, ultraviolet rays, oxygen and other conditions, the epoxy resin molecular chain is broken and decomposed, causing the mechanical properties of the material to gradually decrease. Therefore, how to improve the toughness and aging resistance of epoxy resin after curing has important research significance and application value.

[0003] For example, in the "method of toughening epoxy resin with wollastonite" disclosed in Chinese patent literature, the publication number is CN102532951A. Wollastonite is stirred at 80°C for 30 minutes to improve the reaction activity; wollastonite is wet-modified with silane coupling agent KH-570, and then the modified wollastonite is used to toughen the epoxy resin. When the amount of wollastonite in this method is increased, the toughness of the epoxy resin will begin to decrease, so this method has limited effect on improving the toughness of the epoxy resin. Summary of the invention

[0004] In order to overcome the problem that the prior art has no obvious effect on improving the toughness and aging resistance of epoxy resin after curing, the present invention provides an epoxy resin synergistically toughened by liquid rubber and modified carbon black, and the epoxy resin can maintain good mechanical properties after curing and also has excellent high temperature aging resistance. The present invention also provides a preparation method of the epoxy resin synergistically toughened by liquid rubber and modified carbon black.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] An epoxy resin synergistically toughened by liquid rubber and modified carbon black comprises the following components by weight: 70-100 parts of epoxy resin, 20-30 parts of curing agent, 0.2-1 part of catalyst, 30-60 parts of liquid rubber, 2-10 parts of modified carbon black, 0.25-1 part of antioxidant and 0.25-1 part of ultraviolet absorber.

[0007] The present invention adopts inorganic and organic modifiers to synergistically toughen epoxy resin, so that liquid rubber and modified carbon black form a cross-linked network with an inorganic / organic interface in the epoxy resin. The network has good compatibility with the epoxy resin and good dispersion effect, and can effectively improve the mechanical properties and anti-aging properties of the epoxy resin after curing. It can also reduce the amount of modifier added while achieving the same toughening effect.

[0008] Preferably, the modified carbon black is prepared by the following steps:

[0009] 1) adding high structure carbon black and silane coupling agent into ethanol aqueous solution, heating and stirring to react to obtain silanized carbon black;

[0010] 2) Dissolve the silanized carbon black, initiator and unsaturated fatty acid in toluene, and heat to react to obtain modified carbon black.

[0011] High-structure carbon black itself is chain-like. After unsaturated fatty acids are grafted on its surface, it can avoid self-agglomeration, enhance its compatibility with liquid rubber and epoxy resin, and improve the degree of cross-linking of the network structure formed between it and liquid rubber.

[0012] Preferably, the heating and stirring reaction conditions in step 1) are heating to 55-70° C. and stirring for 4-8 hours, the volume ratio of ethanol to water in the ethanol aqueous solution is (1-3):1, the silane coupling agent is selected from one of KH550, 560, and 570, and the mass ratio of high structure carbon black to silane coupling agent is (2-3):1.

[0013] Preferably, in step 2), the unsaturated fatty acid is selected from one of stearidonic acid and linoleic acid.

[0014] Preferably, in step 2), the initiator is selected from one of azobisisobutyronitrile, azobisisoheptanenitrile and potassium persulfate, the mass ratio of silylated carbon black, initiator and unsaturated fatty acid is 100:(0.1-0.2):(20-50), and the mixture is heated to 45-60° C. and stirred for reaction for 1-3 hours.

[0015] Preferably, the epoxy resin is selected from one of E-51 epoxy resin, E-44 epoxy resin and hydrogenated epoxy resin.

[0016] Preferably, the liquid rubber is selected from one or a combination of double-end functionalized epoxidized polybutadiene rubber, epoxidized nitrile rubber, and epoxidized styrene butadiene rubber, and its double-end functional groups are one of terminal aldehyde groups, terminal hydroxyl groups, terminal carboxyl groups, terminal oxime groups, and terminal primary amine groups.

[0017] The epoxidized liquid rubber has a large number of hydroxyl groups, which is conducive to connecting with modified carbon black.

[0018] Preferably, the curing agent is selected from one or two of modified amine curing agents, low molecular weight polyamide curing agents, imidazole curing agents, phenolic amine curing agents, and acid anhydride curing agents; and the catalyst is selected from one of acid anhydride catalyst BDMA and fatty amine DMP-30.

[0019] Preferably, the antioxidant is selected from one or a combination of antioxidant CA, antioxidant 330, antioxidant MEB, antioxidant 1010, antioxidant 264 and antioxidant 1076; the ultraviolet light absorber is selected from one or a combination of ultraviolet light absorber UV-9, ultraviolet light absorber UVP-327, ultraviolet light absorber UV-531, ultraviolet light absorber UV-P and ultraviolet light absorber RMB.

[0020] A method for preparing an epoxy resin synergistically toughened by liquid rubber and modified carbon black comprises the following steps:

[0021] (1) mixing epoxy resin, liquid rubber, modified carbon black and catalyst, heating to 80-90° C. and stirring for reaction for 1-2 hours to obtain a modified epoxy prepolymer;

[0022] (2) cooling the modified epoxy prepolymer to 30-40° C., adding a curing agent, an antioxidant, and an ultraviolet absorber, and stirring evenly to obtain a rubber compound;

[0023] (3) The rubber material is vacuum degassed at 50-60°C for 15-20 minutes, and then poured into a mold for curing. The curing process is to heat to 90-100°C and keep it warm for 2-2.5 hours, and then heat to 130-150°C and keep it warm for 5-6 hours.

[0024] Therefore, the invention has excellent bending strength, high temperature aging resistance, is not easy to be brittle, has low moisture absorption rate, and is not easy to crack at low temperatures. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with specific implementation methods.

[0026] Example 1

[0027] An epoxy resin synergistically toughened by liquid rubber and modified carbon black, the preparation steps of which are as follows:

[0028] (1) 20 g of high-structure carbon black (Orilon SPECIAL BLACK 4) and 10 g of silane coupling agent KH570 were added to 100 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 2:1), heated to 70 ° C and stirred for 4 h to obtain silanized carbon black, the dried silanized carbon black was added to 150 mL of toluene, 0.03 g of initiator and 4 g of linoleic acid were added, heated to 50 ° C and stirred for 2 h, and filtered to obtain modified carbon black;

[0029] (2) 100 g of E-44 epoxy resin, 35 g of hydroxyl-terminated epoxidized polybutadiene liquid rubber, 10 g of modified carbon black, and 0.25 g of DMP-30 catalyst were mixed, heated to 80° C., stirred and reacted for 1 h to obtain a modified epoxy prepolymer;

[0030] (3) cooling the modified epoxy prepolymer to 30° C., adding 25 g of epoxy resin 593 curing agent, 0.5 g of antioxidant 1010, and 0.5 g of ultraviolet absorber UV-9, and stirring evenly to obtain a rubber compound;

[0031] (4) The adhesive is vacuum degassed at 50°C for 15 min and then poured into a mold for curing. The curing process is to heat to 100°C and keep it for 2 h, then heat to 150°C and keep it for 5 h.

[0032] Example 2

[0033] A liquid rubber and modified carbon black synergistically toughened epoxy resin, which is different from Example 1 in that the amount of terminal hydroxyl epoxidized polybutadiene liquid rubber added in step (2) is 60g.

[0034] Example 3

[0035] An epoxy resin synergistically toughened by liquid rubber and modified carbon black, which differs from Example 1 in that 10 g of octadecatetraenoic acid is used in step (1) to replace linoleic acid.

[0036] Example 4

[0037] A liquid rubber and modified carbon black synergistically toughened epoxy resin, which differs from Example 1 in that in step (2), epoxidized nitrile rubber is used to replace the hydroxyl-terminated epoxidized polybutadiene liquid rubber.

[0038] Comparative Example 1

[0039] An epoxy resin, the preparation steps of which are:

[0040] (1) 145 g of E-44 epoxy resin and 0.25 g of DMP-30 catalyst were mixed, heated to 80° C. and stirred for reaction for 1 h to obtain a modified epoxy prepolymer;

[0041] (2) cooling the modified epoxy prepolymer to 30° C., adding 25 g of epoxy resin 593 curing agent, 0.5 g of antioxidant 1010, and 0.5 g of ultraviolet absorber UV-9, and stirring evenly to obtain a rubber compound;

[0042] (3) The adhesive is vacuum degassed at 50°C for 15 min and then poured into a mold for curing. The curing process is to heat to 100°C and keep it for 2 h, then heat to 150°C and keep it for 5 h.

[0043] Comparative Example 2

[0044] A liquid rubber toughened epoxy resin, the preparation steps of which are:

[0045] (1) 100 g of E-44 epoxy resin, 45 g of hydroxyl-terminated epoxidized polybutadiene liquid rubber, and 0.25 g of DMP-30 catalyst were mixed, heated to 80° C., stirred and reacted for 1 h to obtain a modified epoxy prepolymer;

[0046] (2) cooling the modified epoxy prepolymer to 30° C., adding 25 g of epoxy resin 593 curing agent, 0.5 g of antioxidant 1010, and 0.5 g of ultraviolet absorber UV-9, and stirring evenly to obtain a rubber compound;

[0047] (3) The adhesive is vacuum degassed at 50°C for 15 min and then poured into a mold for curing. The curing process is to heat to 100°C and keep it for 2 h, then heat to 150°C and keep it for 5 h.

[0048] Comparative Example 3

[0049] A modified carbon black toughened epoxy resin, the preparation steps of which are:

[0050] (1) 20 g of high-structure carbon black (Orilon SPECIAL BLACK 4) and 10 g of silane coupling agent KH570 were added to 100 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 2:1), heated to 70 ° C and stirred for 4 h to obtain silanized carbon black, the dried silanized carbon black was added to 150 mL of toluene, 0.03 g of initiator and 4 g of linoleic acid were added, heated to 50 ° C and stirred for 2 h, and filtered to obtain modified carbon black;

[0051] (2) 100 g of E-44 epoxy resin, 45 g of modified carbon black, and 0.25 g of DMP-30 catalyst were mixed, heated to 80° C., stirred and reacted for 1 h to obtain a modified epoxy prepolymer;

[0052] (3) cooling the modified epoxy prepolymer to 30° C., adding 25 g of epoxy resin 593 curing agent, 0.5 g of antioxidant 1010, and 0.5 g of ultraviolet absorber UV-9, and stirring evenly to obtain a rubber compound;

[0053] (4) The adhesive is vacuum degassed at 50°C for 15 min and then poured into a mold for curing. The curing process is to heat to 100°C and keep it for 2 h, then heat to 150°C and keep it for 5 h.

[0054] Comparative Example 4

[0055] An epoxy resin synergistically toughened by liquid rubber and modified carbon black, the preparation steps of which are as follows:

[0056] (1) Add 20 g of high-structure carbon black (Orion SPECIAL BLACK 4) and 10 g of silane coupling agent KH570 to 100 mL of ethanol aqueous solution (the volume ratio of ethanol to water is 2:1), heat to 70° C., stir and react for 4 h to obtain silanized carbon black;

[0057] (2) 100 g of E-44 epoxy resin, 35 g of hydroxyl-terminated epoxidized polybutadiene liquid rubber, 10 g of silanized carbon black, and 0.25 g of DMP-30 catalyst were mixed, heated to 80° C., stirred and reacted for 1 h to obtain a modified epoxy prepolymer;

[0058] (3) cooling the modified epoxy prepolymer to 30° C., adding 25 g of epoxy resin 593 curing agent, 0.5 g of antioxidant 1010, and 0.5 g of ultraviolet absorber UV-9, and stirring evenly to obtain a rubber compound;

[0059] (4) The adhesive is vacuum degassed at 50°C for 15 min and then poured into a mold for curing. The curing process is to heat to 100°C and keep it for 2 h, then heat to 150°C and keep it for 5 h.

[0060] Comparative Example 5

[0061] An epoxy resin synergistically toughened by liquid rubber and modified carbon black, which differs from Example 1 in that the amount of terminal hydroxyl epoxidized polybutadiene liquid rubber added in step (2) is 20 g.

[0062] The mechanical properties, aging resistance and electrical properties of the materials obtained in the above-mentioned embodiments and comparative examples were tested respectively. The mechanical properties test was conducted at room temperature on the samples prepared in the embodiments and comparative examples with reference to GB / T 2567-2008, and at least 3 parallel samples were set up, and the average value was recorded; the high temperature aging test was conducted as follows: the samples prepared in the embodiments and comparative examples were dried at 70°C for 3h, weighed, and then placed at 250°C for 720h for high temperature aging test, and finally weighed after drying at 70°C for 3h, and at least 3 parallel samples were set up, and the mass change rate was calculated, and the average value was recorded. The test results are shown in the following table.

[0063] project Tensile strength(MPa) Bending strength(MPa) <![CDATA[Impact strength (KJ / m 2 )]]> High temperature aging resistance (%) Example 1 106.26 125.2 48.3 1.64 Example 2 117.34 138.2 52.3 1.51 Example 3 100.32 119.1 51.9 1.74 Example 4 94.23 130.1 49.3 2.15 Comparative Example 1 66.89 88.6 21.2 2.45 Comparative Example 2 77.24 98.3 45.8 2.07 Comparative Example 3 89.43 108.5 27.2 1.88 Comparative Example 4 101.52 111.0 42.8 1.52 Comparative Example 5 90.61 101.8 35.5 1.49

[0064] It can be seen from the test data that the present invention significantly improves the mechanical properties and aging resistance of the epoxy resin material after curing.

[0065] From the test data of Example 1 and Comparative Examples 1-3, it can be seen that adding liquid rubber alone or adding modified carbon black alone has a certain toughening effect on epoxy resin, but the effect of the single action is weaker than the synergistic toughening effect of the two. In Comparative Example 4, the carbon black is only modified by silanization, which improves the dispersion effect of carbon black in epoxy resin and prevents it from agglomerating, but the network crosslinking formed by the long chain and liquid rubber on its surface is not sufficient.

[0066] Compared with Comparative Example 5, the increase in toughness of the epoxy resin obtained in Example 2 relative to Example 1 is weaker than the increase in toughness of Example 1 relative to Comparative Example 5. This is because a certain amount of liquid rubber needs to be added to form a network in the epoxy resin, and the toughness of the epoxy resin can be significantly improved after the cross-linked network is formed.

Claims

1. An epoxy resin synergistically toughened by liquid rubber and modified carbon black, characterized in that: The invention comprises the following components by weight: 70-100 parts of epoxy resin, 20-30 parts of curing agent, 0.2-1 parts of catalyst, 30-60 parts of liquid rubber, 2-10 parts of modified carbon black, 0.25-1 parts of antioxidant and 0.25-1 parts of ultraviolet absorber. The modified carbon black is prepared by grafting silanized carbon black with unsaturated fatty acid, and the silanized carbon black is prepared by silanizing carbon black with high-structure carbon black and silane coupling agent. The unsaturated fatty acid is selected from one of octadecadonic acid and linoleic acid. The liquid rubber is selected from one or more of double-end functionalized epoxidized polybutadiene rubber, epoxidized nitrile rubber and epoxidized styrene butadiene rubber, and the double-end functional group is one of terminal aldehyde group, terminal hydroxyl group, terminal carboxyl group, terminal oxime group and terminal primary amine group.

2. The epoxy resin synergistically toughened by liquid rubber and modified carbon black according to claim 1, characterized in that: The modified carbon black is prepared by the following steps: 1) Add high-structure carbon black and silane coupling agent into ethanol aqueous solution, heat and stir to react to obtain silanized carbon black; 2) Dissolve silylated carbon black, initiator and unsaturated fatty acid in toluene and heat to react to obtain modified carbon black.

3. The epoxy resin synergistically toughened by liquid rubber and modified carbon black according to claim 2, characterized in that: The heating and stirring reaction conditions in step 1) are heating to 55-70° C. and stirring for 4-8 hours, the volume ratio of ethanol to water in the ethanol aqueous solution is (1-3):1, the silane coupling agent is selected from one of KH550, 560, and 570, and the mass ratio of high structure carbon black to silane coupling agent is (2-3):

1.

4. The epoxy resin synergistically toughened by liquid rubber and modified carbon black according to claim 2, characterized in that: In the step 2), the initiator is selected from one of azobisisobutyronitrile, azobisisoheptanenitrile and potassium persulfate, the mass ratio of silylated carbon black, initiator and unsaturated fatty acid is 100: (0.1-0.2): (20-50), and the mixture is heated to 45-60° C. and stirred for reaction for 1-3 hours.

5. The epoxy resin synergistically toughened by liquid rubber and modified carbon black according to claim 1, characterized in that: The epoxy resin is selected from one of E-51 epoxy resin, E-44 epoxy resin and hydrogenated epoxy resin.

6. The epoxy resin synergistically toughened by liquid rubber and modified carbon black according to claim 1, characterized in that: The curing agent is selected from one or two of modified amine curing agents, low molecular weight polyamide curing agents, imidazole curing agents, phenolic amine curing agents, and acid anhydride curing agents.

7. The epoxy resin synergistically toughened by liquid rubber and modified carbon black according to claim 1, characterized in that: The catalyst is selected from one of anhydride catalyst BDMA and fatty amine DMP-30.

8. The epoxy resin synergistically toughened by liquid rubber and modified carbon black according to claim 1, characterized in that: The antioxidant is selected from one or more of antioxidant CA, antioxidant 330, antioxidant MEB, antioxidant 1010, antioxidant 264 and antioxidant 1076.

9. The epoxy resin synergistically toughened by liquid rubber and modified carbon black according to claim 1, characterized in that: The ultraviolet absorber is selected from one or a combination of ultraviolet absorber UV-9, ultraviolet absorber UVP-327, ultraviolet absorber UV-531, ultraviolet absorber UV-P and ultraviolet absorber RMB.

10. A method for preparing the epoxy resin synergistically toughened by liquid rubber and modified carbon black as claimed in any one of claims 1 to 9, characterized in that: The steps include: (1) Mix epoxy resin, liquid rubber, modified carbon black and catalyst, heat to 80-90°C, stir and react for 1-2h to obtain modified epoxy prepolymer; (2) Cooling the modified epoxy prepolymer to 30-40°C, adding a curing agent, an antioxidant, and an ultraviolet absorber, and stirring evenly to obtain a rubber compound; (3) Degas the rubber at 50-60℃ in vacuum for 15-20 min, and then pour it into the mold for curing. The curing process is to heat it to 90-100℃ and keep it for 2-2.5 h, and then heat it to 130-150℃ and keep it for 5-6 h.