A composite and a method for preparing the same

Through the nitride layer-transition layer-functional layer composite structure, the wear problem caused by friction between the plunger and the inner holes of the cylinder in the plunger pump is solved, the wear resistance and impact resistance of the plunger are improved, and the service life is extended. and reduce friction and mechanical losses.

CN116162902BActive Publication Date: 2024-11-29JIANGSU XCMG CONSTRUCTION MACHINERY RESEARCH INSTITUTE LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310200185.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-11-29
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

The friction between the plunger and the inner holes of the cylinder in the plunger pump leads to increased wear and leakage. Traditional heat treatment is difficult to meet the service performance requirements under high-speed, high-pressure, and large-displacement conditions, and there are deformation and pore problems in the spraying technology. Laser or ion etching causes residual stress and wear.

Method used

Using a nitride layer-transition layer-functional layer composite structure, including steel matrix, nitriding layer, ZrNb layer, ZrNbN layer, ZrNbCN layer and alternately stacked ZrNb-DLC functional layer, multi-layer structure is formed through ion implantation and arc deposition technology , improve the toughness and impact resistance of the coating.

Benefits of technology

It significantly improves the wear resistance, impact resistance and surface treatment efficiency of the plunger, extends its service life, and shows excellent friction matching with traditional nitriding, copper inlay and ceramic surfaces, reducing friction and mechanical losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116162902B_ABST
    Figure CN116162902B_ABST
Patent Text Reader

Abstract

The present application provides a composite body, including a steel substrate, a nitriding layer grown on the surface of the steel substrate, a transition layer stacked on the nitriding layer, and a functional layer stacked on the transition layer; wherein the transition layer has a multilayer structure, the transition layer includes a ZrNb layer, and a ZrNbN layer stacked on the ZrNb layer; wherein the functional layer has a multilayer structure, the functional layer includes alternately stacked ZrNb layers and DLC layers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of material processing technology, and specifically relates to a composite and a preparation method thereof. Background Art

[0002] The plunger and the inner hole of the cylinder body in the plunger pump form a pair of friction pairs, usually referred to as plunger pairs. As a key component of the plunger pump, the plunger reciprocates in the inner hole of the cylinder body, causing the volume of the sealed working chamber to change to achieve oil suction and oil pressure, and is affected by the bias torque of the slipper during operation. The frequent impact and intense friction between the plunger and the inner hole of the cylinder body can easily cause wear, resulting in increased internal leakage and reduced volumetric efficiency, which reduces the operating efficiency of mechanical equipment. Therefore, surface strengthening of the plunger to improve the wear resistance and impact resistance of the plunger is of great practical significance for improving the reliability of the plunger pump and saving the full life cycle cost.

[0003] Related technologies use carburizing, nitriding or carbonitriding technology to protect the surface of the plunger, and use copper sleeve inlay or hard nitriding technology to protect the surface of the inner hole of the cylinder body. When the oil film breaks, the plunger and the cylinder body show high friction and generate a lot of heat, which can easily lead to plunger wear and burns in the inner hole of the cylinder body. With the development trend of high speed, high pressure and large displacement of plunger pumps, the working conditions in the pump are getting worse and worse. Traditional heat treatment technology has become increasingly difficult to meet the service performance requirements of the plunger. Summary of the invention

[0004] The inventors found that in order to improve the service performance of the plunger pump, the relevant technology uses supersonic flame spraying technology or plasma spraying technology to prepare a ceramic coating on the plunger to reduce the wear between the plunger and the inner hole of the cylinder body. At the same time, the ceramic coating has excellent corrosion resistance and is widely used in the petrochemical industry. For example, Chinese invention patent CN201710566954.2 proposes a method for preparing a long-life coating for a plunger, in which a matrix strengthening layer is obtained by spray welding remelting or surface induction quenching, and a metal-ceramic composite coating is prepared on the basis of the matrix strengthening layer by a supersonic flame thermal spraying process, which solves the defect that traditional plungers cannot meet the growing operating needs of oil and gas fields. Another method to improve the service performance of the plunger is to use laser or ion etching to prepare micro-textures on the plunger surface, which can store hydraulic oil and utilize the microfluidic dynamic pressure effect to improve the lubrication performance of the plunger surface, thereby improving the service reliability of the plunger. For example, Chinese invention patent CN202010204323.8 prepares a groove-pit combined texture on the plunger, which improves the oil film bearing capacity at the friction pair of the plunger, reduces friction and end leakage, reduces mechanical losses, and improves volumetric efficiency.

[0005] The inventors found that the use of spraying technology to prepare a ceramic coating reinforced plunger can easily lead to large deformation of the plunger, and the generation of pores cannot be avoided during the spraying process. It is usually necessary to grind the sprayed surface before sealing the pores, which has the problems of complex procedures and high costs. The use of laser or ion etching to prepare a micro-texture with a micro-fluid pressure effect on the plunger surface will lead to the generation of residual stress and micro-cracks. The micro-texture cannot change the lubrication properties of the material itself and is prone to wear. After the texture is worn, the lubrication of the plunger fails.

[0006] In view of the problems that the existing technology is difficult to meet the service performance requirements of the plunger, and the process is cumbersome and inefficient, the present invention provides a high wear-resistant and impact-resistant coating for plunger surface protection and a preparation method thereof. The coating can greatly improve the wear resistance and impact resistance of the plunger. The method can improve the surface treatment efficiency of the plunger. The plunger with the coating has high reliability and can improve the service life under alternating loads.

[0007] In a first aspect, the present invention provides a composite body, comprising a steel substrate, a nitriding layer grown on the surface of the steel substrate, a transition layer stacked on the nitriding layer, and a functional layer stacked on the transition layer;

[0008] Wherein, the transition layer has a multi-layer structure, and the transition layer includes a ZrNb layer and a ZrNbN layer stacked on the ZrNb layer;

[0009] The functional layer has a multi-layer structure, and includes alternately stacked ZrNb layers and DLC layers.

[0010] In the above-mentioned implementation scheme, the composite structure of nitride layer-transition layer-functional layer proposed in the present invention has strong toughness and the ability to resist frequent impact deformation on the basis of ensuring the bonding force between the coating and the substrate.

[0011] In the above scheme, the nitride layer-transition layer-functional layer composite structure has high bonding strength, high wear resistance and high toughness, and has a long service life under high impact and high load conditions.

[0012] In the above scheme, the functional layer adopts the soft and hard alternating form of zirconium-niobium alloy-zirconium-niobium doped DLC, which can buffer stress and improve the overall toughness of the coating, giving the coating wear resistance and impact resistance.

[0013] In some embodiments, the transition layer further includes a ZrNbCN layer stacked on the ZrNbN layer.

[0014] In some embodiments, the layer of the functional layer closest to the steel substrate is a DLC layer.

[0015] In some embodiments, the layer of the functional layer farthest from the steel substrate is a DLC layer.

[0016] In some embodiments, the functional layer includes n DLC layers and n-1 ZrNb layers, where n=10-20.

[0017] In some embodiments, the DLC layer is doped with Nb and Zr elements.

[0018] In some embodiments, the thickness of the nitrided layer is 0.1-0.2 μm.

[0019] In some embodiments, the transition layer has a thickness of 0.4 to 0.6 μm.

[0020] In some embodiments, the thickness of the functional layer is 1 to 3 μm.

[0021] In some embodiments, the total thickness of the nitriding layer, the transition layer and the functional layer of the composite is 1.5 to 3.8 μm.

[0022] In some embodiments, the material of the steel matrix includes one or more of the following: 20Cr3MoWV steel, 42CrMo steel, 38CrMoAlA steel, 31CrMoV9 steel, 20Cr steel, and 40Cr steel.

[0023] In some embodiments, the composite body is a friction pair component.

[0024] In some embodiments, the composite body is a hydraulic pump friction part.

[0025] In some embodiments, the complex is selected from one or more of the following: a hydraulic pump motor plunger, a swash plate, and a return plate.

[0026] In some embodiments, the composite body is a plunger having the above-mentioned impact-resistant and high-wear-resistant coating, which has excellent friction adaptability and exhibits excellent friction matching with existing nitrided, copper-inlaid, ceramic and other cylinder inner hole surface layers, and can significantly improve the reliability of the plunger pair.

[0027] In some embodiments, the composite is selected from one or more of the following: hydraulic components, fuel components.

[0028] In some embodiments, the composite is selected from one or more of the following: a gear pump component, a vane pump component, a hydraulic valve component, and an automobile fuel pump component.

[0029] In some embodiments, the surface of the composite has one or more of the following characteristics:

[0030] (1) Surface hardness is 1200~1500HV;

[0031] (2) Surface roughness is less than Ra0.2μm;

[0032] (3) The bonding strength of the nitriding layer, transition layer and functional layer is above 80N.

[0033] In a second aspect, the present invention provides a method for preparing any of the above-mentioned complexes, comprising:

[0034] (1) Providing a steel substrate;

[0035] (2) nitriding the steel substrate by ion implantation technology to form a nitriding layer;

[0036] (3) using arc deposition technology to prepare ZrNb and ZrNbN layers to form a gradient layer;

[0037] (4) Arc deposition technology is used to alternately prepare ZrNb layers and DLC layers to form a functional layer.

[0038] In some embodiments, step (3) further comprises: preparing the ZrNbCN layer using arc deposition technology.

[0039] In the above scheme, the ion implantation of metal for nitriding treatment can quickly improve the surface hardness of the base material and quickly establish effective support for the deposition of the composite coating.

[0040] In the above scheme, the gradient transition layer is prepared by using filtered arc composite pulse arc technology, which can alleviate the difference in material mechanical properties between the periodic functional layer and the substrate and ensure the bonding force between the layer and the substrate.

[0041] In the above scheme, the ion implantation technology is combined with the PVD technology (pulse arc technology and filtered arc technology), which improves the surface treatment efficiency of the plunger and reduces the surface treatment cost of the plunger.

[0042] In some embodiments, magnetron sputtering and DC arc technology can be used to excite metal targets and graphite targets.

[0043] In some embodiments, the method for preparing the composite body includes the operation of machining a steel substrate, specifically including: subjecting the steel substrate to a quenching and tempering treatment, and then machining the steel substrate to obtain the required external dimensions of the sample.

[0044] In some embodiments, the method for preparing the composite includes an ultrasonic cleaning operation, which specifically includes: firstly, rinsing the sample with a metal cleaning agent to remove grease, metal debris, etc. remaining from the surface machining process, and then ultrasonically cleaning the sample with deionized water, anhydrous alcohol, and gasoline solvent to remove microscopic impurities and other attachments on the surface of the sample, and then drying with nitrogen and placing in a blast drying oven for standby use;

[0045] In some embodiments, the method for preparing the composite includes a glow cleaning operation, specifically comprising: placing the sample into a vacuum chamber, adjusting the rotating frame speed to 2 to 3 r / min, and drawing the vacuum to 5×10 -3 Pa, the vacuum chamber is heated to 300℃ and kept warm for 15min, argon is introduced, the vacuum chamber pressure is maintained at 2-4Pa, the pulse bias is 800-1000V, the frequency is 20KHz, the duty cycle is 0.2, and the sample is cleaned for 15-20min;

[0046] In some embodiments, the method for preparing a composite body includes the operation of preparing a nitriding layer, specifically including: turning off argon gas, introducing nitrogen gas into the pipeline of the anode layer ion source, the pressure is 0.1-0.3 Pa, adjusting the temperature to 450° C., the bias voltage is 20-30 KV, the duty cycle is 0.5, turning on the ion source, the voltage is 650-850 V, the duty cycle is 0.4-0.6, and nitrogen ions are implanted into the surface of the workpiece for 3-4 hours to obtain a nitriding layer;

[0047] In some embodiments, the method for preparing the composite includes the operation of preparing the transition layer, specifically including: turning off nitrogen and ion source, adjusting the bias voltage to 100-200V, the duty cycle to 0.8, the temperature to 200°C, the arc current of the magnetic filtered arc source 5 to 50-55A, the arc current of the magnetic filtered arc source 7 to 70-75A, and depositing the ZrNb alloy layer for 5-10 minutes; slowly introducing nitrogen, the pressure is uniformly increased from 0 to 0.3Pa within 10 minutes, and the ZrNbN layer is deposited; adjusting the working power supply of the pulse arc source 6 to 280-320V, the frequency is increased from 1Hz to 15Hz within 15 minutes, and the step amplitude per minute is 1Hz, and the ZrNbCN layer is deposited, thereby obtaining a ZrNb-ZrNbN-ZrNbCN gradient transition layer;

[0048] In some embodiments, the method for preparing the composite includes the operation of preparing the functional layer, specifically including: turning off the nitrogen, adjusting the bias voltage to 100V, the frequency of the pulse arc source 6 to 10Hz, the current of the magnetic filtering arc source 5 to 50A, the current of the magnetic filtering arc source 7 to 60A, depositing the Nb and Zr co-doped DLC layer for 8-10min, then turning off the pulse arc source 6, keeping the arc currents of the magnetic filtering arc sources 5 and 7 unchanged for 2-4min, depositing the ZrNb alloy layer, repeating the above steps 10-20 times, obtaining a periodic, soft and hard alternating ZrNb-DLC functional layer, the total number of functional layers is an odd number (≥21), wherein both ends are Nb and Zr co-doped DLC layers;

[0049] In some embodiments, the method for preparing a composite includes a cooling tank, specifically comprising: taking out the sample after the vacuum chamber is cooled to room temperature.

[0050] In a third aspect, the present invention provides a coating device for preparing any of the above-mentioned composite bodies, the device comprising:

[0051] The composite coating device integrates a pulse arc source, a magnetic filter arc source, and an anode layer ion source into a vacuum chamber;

[0052] The pulse arc, magnetically filtered arc source and anode layer ion source have a common sputtering area.

[0053] In some embodiments, the pulse arc source is vertically mounted on the side wall of the vacuum chamber, with the central axis intersecting with the central axis of the workpiece turret, and the target material of the pulse arc source is high-purity graphite.

[0054] In some embodiments, the magnetic filtered arc source is a curved tube filtered arc source, which is vertically mounted on the side wall of the vacuum chamber, symmetrically distributed on both sides of the pulse arc source, and at the same height as the pulse arc source. The targets of the pulse arc source are high-purity Zr target and high-purity Nb target, respectively.

[0055] In some embodiments, the elbow filtering is 60°-120°, for example a 90° change.

[0056] In some embodiments, the Nb target and the Zr target can be replaced by a ZrNb alloy target. In some embodiments, the graphite target can be replaced by a ZrNbC composite target.

[0057] In some embodiments, the anode layer ion source is vertically mounted on the side wall of the vacuum chamber, with its central axis intersecting with the central axis of the workpiece turret and at the same height as the pulse arc source.

[0058] In the above scheme, the present invention integrates three technologies of pulse arc, filtered arc and ion beam into one, which can realize the doping of various metal and non-metal elements and the precise control of the doping element content and film performance, and has strong scientific research and application value.

[0059] Terminology Note:

[0060] The term "nitriding" refers to a chemical heat treatment process that allows nitrogen atoms to penetrate into the surface of a workpiece in a certain medium at a certain temperature. Common methods include liquid nitriding, gas nitriding, and ion nitriding. Nitriding a steel matrix can form a nitriding layer. According to the Fe-N phase diagram, the structures of the nitriding layer from the surface to the inside are nitride layer, nitride + nitrogen-containing α, and nitrogen-containing α.

[0061] Ion nitriding is the process of infiltrating nitrogen atoms into a steel matrix by ion implantation. Ion implantation is the process of ionizing the required gas or solid vapor in a vacuum system, extracting an ion beam, and then directly injecting it into the material at an acceleration of several thousand electron volts to several hundred thousand electron volts to a certain depth, thereby changing the composition and structure of the material surface and achieving the purpose of improving performance.

[0062] DLC layer (Diamond-like carbon (DLC) coating). The diamond-like layer has properties similar to diamond, so it is called diamond-like carbon layer, or DLC layer for short. The arrangement of C atoms in the DLC structure is very similar to the popular amorphous structure, but it is mixed with polycrystalline and diamond or single crystal clusters, which makes it have some properties similar to crystalline diamond, but it is different from the crystal structure of natural corundum.

[0063] The pulse arc technology for producing DLC ​​layer uses solid graphite as the target material. A vacuum arc is used to excite the graphite target material to generate carbon ions, which are deposited on the surface of the workpiece to form a DLC film.

[0064] DLC layer can also be prepared by ion beam method, such as DIBSD method: Ar + Ion beam sputtering of graphite target produces sputtered C atoms that are deposited on the bottom surface. In the process of producing and growing completely disordered C film, Ar with energy in the range of 1000eV is applied. + Auxiliary macro, through the non-reflection enhanced DIBSD process, the unnecessary C is transformed into a metastable DLC film. Another example is the direct ion beam deposition method. CH compound gas or a mixed gas with Ar gas is introduced into the ion source, and the CH compound gas is ionized in the ion source discharge chamber to generate C with a certain energy. + Ions bombard the substrate. As long as C +The arrival rate of ions is higher than the re-sputtering rate of deposited C atoms, which generates condensed C atoms on the substrate. During the condensation process, they are bombarded by the same ion beam, and the deposited C atoms form a DLC structure through the ion heat peak process. Both methods can deposit DLC films with similar physical properties.

[0065] The DLC layer may be doped with Zr element, with the doping amount being 30000-60000 ppm, preferably 40000-50000 ppm.

[0066] The DLC layer may be doped with Nb element, with the doping amount being 5000-15000 ppm, preferably 8000-10000 ppm.

[0067] The material of the term “ZrNb layer” is ZrNb alloy, and the mass ratio of Zr to Nb is 6-8:12-14, for example 7:13.

[0068] The material of the term "ZrNbN layer" is ZrNbN alloy, and the mass ratio of Zr, Nb and N is 5-7:9-11:1, for example 6:10:1

[0069] The material of the term “ZrNbCN layer” is ZrNbCN alloy, and the mass ratio of Zr, Nb, C and N is 7-9:11-13:0.8-1.2:0.8-1.2, for example, 8:12:1:1.

[0070] Beneficial effects of this application:

[0071] One or more technical solutions of the present invention have one or more of the following beneficial effects:

[0072] (1) The nitride layer-transition layer-functional layer composite structure proposed in the present invention has strong toughness and the ability to resist frequent impact deformation while ensuring the bonding strength between the coating and the substrate.

[0073] (2) The nitride layer and transition layer can alleviate the difference in mechanical properties between the surface functional layer and the plunger base material, and improve the bonding strength and bearing capacity of the functional layer.

[0074] (3) The functional layer adopts [ZrNb-DLC]n with periodic alternation of soft and hard layers, which has both strong toughness and high hardness, and can significantly improve the wear resistance and impact resistance of the plunger. The DLC layer can be doped with Zr and Nb bimetallic elements, which further improves the toughness of DLC itself and ensures a close bond with the ZrNb alloy layer.

[0075] (4) The composite of the present invention exhibits super strong friction adaptability as a plunger. When the inner hole of the cylinder body is nitrided, copper-plated or ceramic, the plunger of the present invention exhibits excellent friction matching with the inner hole of the cylinder body, which can greatly improve the reliability of the plunger pair.

[0076] (5) The present invention integrates three technologies, namely pulse arc, filtered arc and ion beam, into one, which can realize the doping of various metal and non-metal elements and the precise control of the doping element content and film performance, and has strong scientific research and application value.

[0077] (6) Combining ion implantation with pulse arc and filtered arc technology and applying them to plunger surface treatment greatly shortens the plunger surface treatment time and improves the plunger surface treatment efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0078] Figure 1 A schematic diagram of a complex of the present invention is shown.

[0079] Figure 2 A film coating device according to the present invention is shown.

[0080] Figure 3 A flow chart showing a method for preparing a composite according to the present invention.

[0081] Figure 4 (a) shows a friction pair and a cylindrical specimen of Example 1.

[0082] Figure 4 (b) shows a friction pair and a cylindrical specimen of Comparative Example 1.

[0083] Figure 5 The curve showing the change of friction coefficient of the sample with time in the wear test. DETAILED DESCRIPTION

[0084] The specific embodiments of the present application will now be mentioned in detail. Although the present application is described in conjunction with these specific embodiments, it should be appreciated that it is not intended to limit the present application to these specific embodiments. On the contrary, these embodiments are intended to cover substitutions, changes or equivalent embodiments that may be included in the spirit and scope of the invention defined by the claims. In the following description, a large number of specific details are set forth in order to provide a comprehensive understanding of the present application. The present application can be implemented without some or all of these specific details. In other cases, in order not to make the present application unnecessarily obscure, well-known process operations are not described in detail.

[0085] When used in conjunction with "including," "methods comprising," or similar language in this specification and the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs.

[0086] Unless otherwise specified, the experimental conditions used in the examples of this application are conventional experimental conditions in the art. Unless otherwise specified, the reagents used in the examples of this application are commercially available.

[0087] Figure 1 A schematic diagram of a composite body of the present invention is shown. As shown in the figure, the composite body includes a steel substrate 50, a nitriding layer 10 grown on the surface of the steel substrate 50, a transition layer 20 stacked on the nitriding layer 10, and a functional layer 30 stacked on the transition layer 20;

[0088] The transition layer 20 has a multi-layer structure, and includes a ZrNb layer 21, a ZrNbN layer 22 stacked on the ZrNb layer 21, and a ZrNbCN layer 23 stacked on the ZrNbN layer 22;

[0089] The functional layer 30 has a multi-layer structure, and includes ZrNb layers 32 and DLC layers 31 that are alternately stacked.

[0090] Figure 2 A coating device of the present invention is shown, which comprises: a vacuum chamber 1, a heating system 2, an exhaust system 3, a pulse bias system 4, a pulse arc source 6, a magnetic filter arc source (5, 7), a gas distribution system 8, an anode layer ion source 9 and a workpiece rotating rack 10, wherein:

[0091] The pulse arc source 6 is vertically mounted on the side wall of the vacuum chamber 1, with its central axis intersecting with the central axis of the workpiece rotating rack 10, and the target material of the pulse arc source 6 is high-purity graphite;

[0092] The magnetic filtering arc source (5, 7) is a 90° elbow filtering arc source, which is vertically mounted on the side wall of the vacuum chamber 1 and symmetrically distributed on both sides of the pulse arc source 6, and is at the same height as the pulse arc source 6. The target materials of the pulse arc source (5, 7) are respectively a high-purity Zr target material and a high-purity Nb target material;

[0093] The anode layer ion source 9 is vertically mounted on the side wall of the vacuum chamber 1, with its central axis intersecting with the central axis of the workpiece rotating rack 10, and is at the same height as the pulse arc source 6;

[0094] The pulse arc 6, magnetically filtered arc sources 5 and 7, and anode layer ion source 9 have a common sputtering area;

[0095] The above-mentioned coating device integrates a pulse arc source, a magnetically filtered arc source, and an anode layer ion source in a vacuum chamber, and can realize multiple coating functions. For example, it can prepare Zr, Nb metal single substance thin films, ZrNb double alloy thin films, ZrC, ZrNbC, ZrNbN, ZrNbCN and other ceramic thin films, and multi-doped diamond-like thin films on the substrate surface.

[0096] Figure 3 The flow chart of the method for preparing the composite is shown. As shown in the figure, the preparation method includes the following steps: (S1) machining; (S2) ultrasonic cleaning; (S3) glow cleaning; (S4) preparation of nitriding layer; (S5) preparation of transition layer; (S6) preparation of functional layer; (S7) cooling. The following is a detailed discussion in conjunction with specific embodiments.

[0097] Example 1

[0098] The method for preparing the composite body using the above-mentioned coating device is as follows:

[0099] (S1) Mechanical processing: The steel substrate (38CrMoAlA) was subjected to quenching and tempering treatment, and then subjected to mechanical processing such as turning, outer diameter grinding, ball head grinding and superfine grinding to obtain the required outer dimensions (cylindrical, diameter 32 mm) and surface roughness (Ra 0.2 μm) of the specimen;

[0100] (S2) Ultrasonic cleaning: First, the sample is rinsed with a metal cleaning agent to remove grease, metal debris, etc. remaining from the surface machining process, and then the sample is ultrasonically cleaned for 30 minutes using deionized water, anhydrous alcohol, and gasoline solvent to remove microscopic impurities and other attachments on the surface of the sample. After drying with nitrogen, the sample is placed in a blast drying oven for standby use;

[0101] (S3) Glow cleaning: Place the sample in the vacuum chamber, adjust the rotating speed to 2-3 r / min, and draw the vacuum to 5×10 - 3 Pa, the vacuum chamber is heated to 300℃ and kept warm for 15min, argon is introduced, the vacuum chamber pressure is maintained at 2-4Pa, the pulse bias is 800-1000V, the frequency is 20KHz, the duty cycle is 0.2, and the sample is cleaned for 15-20min;

[0102] (S4) Preparation of nitriding layer: turn off argon gas, introduce nitrogen gas into the pipeline of the anode layer ion source, the pressure is 0.1-0.3 Pa, adjust the temperature to 450° C., bias voltage is 20-30 KV, duty cycle is 0.5, turn on the ion source, voltage is 650-850 V, duty cycle is 0.4-0.6, and nitrogen ions are implanted into the workpiece surface for 3-4 hours to obtain a nitriding layer;

[0103] (S5) Preparation of transition layer: turn off nitrogen and ion source, adjust bias voltage to 100-200V, duty cycle to 0.8, temperature to 200°C, arc current of magnetic filter arc source 5 to 50-55A, arc current of magnetic filter arc source 7 to 70-75A, deposit ZrNb alloy layer for 5-10min; slowly introduce nitrogen, increase pressure from 0 to 0.3Pa uniformly within 10min, deposit ZrNbN layer; adjust working power supply of pulse arc source 6 to 280-320V, increase frequency from 1Hz to 15Hz within 15min, step amplitude per minute to 1Hz, deposit ZrNbCN layer, thereby obtaining ZrNb-ZrNbN-ZrNbCN gradient transition layer;

[0104] (S6) Preparation of functional layer: turn off nitrogen, adjust bias voltage to 100V, frequency of pulse arc source 6 to 10Hz, current of magnetic filtering arc source 5 to 50A, current of magnetic filtering arc source 7 to 60A, deposit Nb and Zr co-doped DLC layer for 8-10min, then turn off pulse arc source 6, keep arc currents of magnetic filtering arc sources 5 and 7 unchanged for 2-4min, deposit ZrNb alloy layer, repeat the above steps 10-20 times, obtain periodic, soft and hard alternating ZrNb-DLC functional layer, the total number of functional layers is an odd number (≥21), both ends of which are Nb and Zr co-doped DLC layers;

[0105] (S7) Cooling: After the vacuum chamber cools to room temperature, the sample is taken out.

[0106] Table 1

[0107]

[0108]

[0109] Comparative Example 1

[0110] (S1) Plunger machining: The steel substrate (38CrMoAlA) is subjected to quenching and tempering treatment, and then subjected to machining such as turning, outer diameter grinding, ball head grinding, and superfine grinding to obtain the required outer dimensions (cylindrical, diameter 32 mm) and surface roughness (Ra 0.2 μm) of the plunger;

[0111] (S2) Pre-ultrasonic cleaning of the plunger: First, the plunger is rinsed with a metal cleaning agent to remove grease, metal debris, etc. remaining during the surface machining process, and then the plunger is ultrasonically cleaned for 30 minutes using deionized water, anhydrous alcohol, and gasoline solvent to remove microscopic impurities and other attachments on the surface of the plunger. After being blown dry with nitrogen, the plunger is placed in a blast drying oven for standby use;

[0112] (S3) Plunger glow cleaning: Place the plunger into the vacuum chamber, adjust the rotating frame speed to 2-3 r / min, and draw the vacuum to 5×10-3 Pa, the vacuum chamber is heated to 300℃ and kept warm for 15min, argon is introduced, the vacuum chamber pressure is maintained at 2-4Pa, the pulse bias is 800-1000V, the frequency is 20KHz, the duty cycle is 0.2, and the plunger is cleaned for 15-20min;

[0113] (S4) Preparation of nitriding layer: turn off argon gas, introduce nitrogen into the pipeline of the anode layer ion source, the pressure is 0.1-0.3Pa, adjust the temperature to 450°C, bias to 20-30KV, duty cycle to 0.5, turn on the ion source, voltage to 650-850V, duty cycle to 0.4-0.6, perform nitrogen ion implantation on the workpiece surface for 3-4h to obtain a nitriding layer (depth 0.4mm).

[0114] Analysis and testing

[0115] (1) Hardness test

[0116] Refer to ASTM E384-2017 Standard Test Method for Microindentation Hardness of Materials

[0117] (2) Binding strength test

[0118] Refer to ISO 20502-2005 Fine ceramics (advanced ceramics, advanced technical ceramics). Determination of adhesion of ceramic coatings by scratch test

[0119] (3) Surface roughness

[0120] Refer to GB / T 31227-2014 Method for measuring surface roughness of sputtered films using atomic force microscope

[0121] (4) Friction pair matching test

[0122] The friction pair matching test under oil lubrication conditions was carried out using an MMW-2 friction and wear testing machine. The hydraulic oil was XCMG AE46 hydraulic oil, the loading pressure was 2000N, the speed was 1000r / min, and the experimental time was 4h.

[0123] Figure 4 (a) shows a friction pair (tin bronze ring specimen) and the cylindrical specimen of Example 1. Figure 4 (b) shows a friction pair (tin bronze ring specimen) and the cylindrical specimen of Comparative Example 1.

[0124] Figure 5 The curves showing the change of friction coefficient over time of the samples of Example 1 and Comparative Example 1 in the wear test are shown.

[0125] The test results show that:

[0126] hardness Binding force Roughness Friction coefficient Wear weight loss Example 1 1245HV 85N Ra0.17μm 0.17 0.012g Comparative Example 1 750HV / Ra0.19μm 0.28 0.04g

[0127] The plunger pump plunger with a high wear-resistant and impact-resistant coating prepared by the present invention has a nitriding layer, a ZrNb-ZrNbN-ZrNbCN gradient transition layer and a [ZrNb-DLC]n periodic functional layer in sequence from the substrate surface to the outside, and the surface hardness reaches 1200-1500 HV, which is at least 1 times higher than that of traditional processes such as nitriding and carburizing. The bonding force between the coating and the substrate reaches more than 80N, the coating thickness is 1.5-3.8μm, and the surface roughness is below Ra0.17μm.

[0128] like Figure 4 As shown, the sample of comparative example 1 was sintered, and the sample of embodiment 1 had only slight wear on the copper.

[0129] like Figure 5 As shown, compared with Comparative Example 1, the friction coefficient of Example 1 is only 0.17, which is 33.3% lower than that of Comparative Example 1, and the abrasion weight loss of the sample of Example 1 is only 0.012 g, which is 70% lower than that of Comparative Example 1.

[0130] The coating preparation method of the present invention is not only applicable to plungers, but also to other hydraulic pump friction parts such as swash plates and return plates. It can improve the comprehensive service performance of plunger pumps under complex and harsh working conditions and has extremely high industrial promotion and application value.

[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit it. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present application can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present application, which should be included in the scope of the technical solution for protection in the present application.

Claims

1. A composite body comprising a steel substrate, a nitriding layer grown on the surface of the steel substrate, a transition layer stacked on the nitriding layer, and a functional layer stacked on the transition layer; in, The transition layer has a multi-layer structure, and the transition layer includes a ZrNb layer, a ZrNbN layer stacked on the ZrNb layer, and a ZrNbCN layer stacked on the ZrNbN layer; The functional layer has a multilayer structure, and includes alternately stacked ZrNb layers and DLC layers. The surface of the composite body has: a surface hardness of 1200-1500 HV and a surface roughness of Ra 0.2 μm or less; and the bonding force of the nitriding layer, the transition layer and the functional layer is above 80N. 2 . The composite body according to claim 1 , wherein the layer closest to the steel substrate in the functional layer is a DLC layer. 3 . The composite body according to claim 1 , wherein the layer of the functional layer farthest from the steel substrate is a DLC layer. 4 . The composite body according to claim 1 , wherein the functional layer comprises n DLC layers and n-1 ZrNb layers, where n=10-20. The composite body according to claim 1 , wherein the DLC layer is doped with Nb and Zr elements. The composite body according to claim 1 , wherein the thickness of the nitrided layer is 0.1 to 0.2 μm. The composite according to claim 1 , wherein the thickness of the transition layer is 0.4 to 0.6 μm.

8. The composite according to claim 1, wherein: The thickness of the functional layer is 1-3 μm.

9. The composite according to claim 1, wherein: The sum of the thickness of the nitriding layer, transition layer and functional layer is 1.5~3.8μm.

10. The composite body according to claim 1, wherein the material of the steel matrix comprises one or more of the following: 20Cr3MoWV steel, 42CrMo steel, 38CrMoAlA steel, 31CrMoV9 steel, 20Cr steel, 40Cr steel.

11. The composite body according to claim 1, which is a friction pair component.

12. A method for preparing the composite according to any one of claims 1 to 11, comprising: (1) Providing a steel substrate; (2) Using ion implantation technology to nitride the steel substrate to form a nitriding layer; (3) Using arc deposition technology to prepare ZrNb layer, ZrNbN layer and ZrNbCN layer to form a transition layer; (4) Arc deposition technology is used to alternately prepare ZrNb layers and DLC layers to form a functional layer.

Citation Information

Patent Citations

  • Composite coating plunger long in service life and applicable to plunger pumps

    CN109253080A

  • Axial plunger pump with groove-pit combined type texture

    CN111237152A

  • Composite film plating device

    CN112522677A

  • Method of obtaining multilayer wear-resistant diamond-like coatings

    RU2740591C1

  • Heat treatable coated article with zirconium silicon oxynitride layer(s) and methods of making same

    US20060159933A1