A powder metallurgy parking limit block and production method thereof

Through the powder metallurgy process, including batching, pressing, sintering, drilling and quenching, the problems of low production efficiency and low precision of the existing parking limit blocks are solved, and efficient and stable parking limit block production is achieved, eliminating the need for Safety hazards are eliminated and safe use requirements are met.

CN116174720BActive Publication Date: 2024-10-29LAIWU IRON & STEEL GRP POWDER METALLURGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211392975.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-08
Publication Date
2024-10-29
Estimated Expiration
2042-11-08

AI Technical Summary

Technical Problem

Due to the complex structure and high requirements on internal surface finish and angle, the existing parking limit block production process has low production efficiency, low precision, low yield rate, and safety hazards, and cannot fully meet the requirements for safe use.

Method used

Using powder metallurgy technology, including batching, pressing, sintering, drilling and quenching, processing through alloy drills and milling cutters, combined with vibration grinding and oil immersion treatment, the powder metallurgy parking limit block with high density and good hole channel accuracy is produced .

Benefits of technology

It improves production efficiency, improves the accuracy, yield rate, stability and safety of the parking limit block, meets the requirements for safe use, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116174720B_ABST
    Figure CN116174720B_ABST
Patent Text Reader

Abstract

The present invention provides a production method of a powder metallurgy parking stop block, comprising: batching, pressing, sintering, drilling, and quenching; the batching comprises uniformly mixing iron powder, copper powder, and graphite to obtain a mixture; the mixture is pressed and formed, and then sintered to obtain a sintered part; the sintered part is drilled and quenched to obtain a powder metallurgy parking stop block. The present invention also provides a powder metallurgy parking stop block, which contains, by mass%, C 0.2-1.0%, Cu 1.0-5.0%, and the remainder is Fe and unavoidable impurities, and the density is >6.8g / cm 3 The present invention effectively overcomes the problems of the prior art in producing the parking limit block of the specific structure of the present invention, which is difficult to manufacture, has low production efficiency and high comprehensive production cost due to the aforementioned complex structure, high requirements for inner surface finish and angle, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of parking limit blocks, in particular to a powder metallurgy parking limit block and a production method thereof. Background Art

[0002] With the continuous development of science and technology, the requirements for motor vehicle parking systems are getting higher and higher. Traditional parking devices usually need to cooperate with handbrake levers, parking limit blocks and other mechanisms to achieve the parking limit of motor vehicles.

[0003] Powder metallurgy parts have good physical and mechanical properties, high design flexibility and low production cost, so they are widely used in the field of motor vehicles. Powder metallurgy parts are used in key parts of motor vehicles such as motor vehicle chassis, brake system, fuel pump, oil pump, engine, transmission and brake booster vacuum pump. Especially in recent years, with the rapid development of the motor vehicle industry, more and more parts are designed to be produced by powder metallurgy process in order to reduce the production cost of motor vehicles while ensuring performance.

[0004] In the prior art, the production process of existing parking limit blocks is usually to use a machining center to perform milling and drilling after precision casting. However, the structure of the existing parking limit block is relatively complex, and it needs to slide relative to the parking mating part to achieve the desired parking limit effect. The smoothness and angle of the inner surface of the parking limit block cannot fully meet the process requirements when processed by the existing process.

[0005] At present, the existing parking limit block production process is difficult to manufacture due to the aforementioned complex structure, high requirements for inner surface finish and angle, etc., with low production efficiency and high comprehensive production cost. At the same time, the parking limit block produced by the existing parking limit block production process has low precision, low yield rate, and cannot be effectively improved. The product reliability is poor, and it is seriously worn during actual use. There are safety hazards and it cannot fully meet the safety use requirements. Summary of the invention

[0006] In order to solve the technical problems existing in the prior art, the present invention provides a powder metallurgy parking limit block and a production method thereof, which can effectively improve the production efficiency on the basis of ensuring the smoothness and angle requirements of the inner surface of the parking limit block; the prepared parking limit block has high precision, effectively improves the yield rate, and the product performance is stable, effectively eliminates safety hazards, and can meet the requirements of safe use.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0008] A method for producing a powder metallurgy parking limit block, comprising: batching, pressing, sintering, drilling, and quenching;

[0009] The ingredients are mixed uniformly with iron powder, copper powder and graphite to prepare a mixture;

[0010] The mixed material is pressed and formed, and then sintered to obtain a sintered part; the sintered part is drilled and quenched to obtain a powder metallurgy parking limit block;

[0011] The powder metallurgy parking limit block contains, by mass%, 0.2-1.0% C, 1.0-5.0% Cu, and the remainder Fe and unavoidable impurities.

[0012] Furthermore, the pressing adopts an upper and a lower powder forming die frame to press the mixture to form a blank; the density of the blank is 6.85-6.95g / cm 3 .

[0013] Furthermore, the pressing pressure is 30-32T, the demoulding pressure is 15-17T, and the powder addition amount of the mixture is 2-2.2 times of the mold volume.

[0014] Furthermore, the sintering temperature is 1110-1130° C. and the sintering time is 40-50 minutes.

[0015] Furthermore, the drilling is performed on the sintered part using a machining center;

[0016] The drilling is performed using an alloy drill bit and a milling cutter;

[0017] For the drilling, the spindle speed of the machining center is 5000-6000rpm.

[0018] Furthermore, the quenching is to sequentially quench and temper the sintered part after drilling, and then vibrate grind and immerse in oil to obtain a powder metallurgy parking limit block;

[0019] The quenching temperature is 810-830°C, and the tempering temperature is 180-190°C;

[0020] The quenching and tempering treatment time is 1-1.2h;

[0021] The vibration grinding has a power of 3.5-5KW and a vibration grinding time of 60-70min.

[0022] A powder metallurgy parking limit block, made by the above production method;

[0023] The powder metallurgy parking limit block comprises: a semicircular inner hole and a positioning wall;

[0024] The semicircular inner hole is in a hollow semicircular arc shape, and includes: a first inner hole area and a second inner hole area;

[0025] The first inner hole area and the second inner hole area are connected by a step transition; the step is a smooth step slope;

[0026] The positioning wall is arranged on the opposite side of the semicircular inner hole accommodating space and is integrally formed with the outer wall of the semicircular inner hole;

[0027] The positioning wall is provided with a positioning hole for fixing the powder metallurgy parking limit block at a predetermined position.

[0028] Further, the outer diameter of the first inner hole region is equal to the outer diameter of the second inner hole region;

[0029] The inner diameter of the first inner hole region is greater than the inner diameter of the second inner hole region.

[0030] Furthermore, the ratio of the inner diameters of the first inner hole region to the second inner hole region is 1.05-1.1:1.

[0031] Furthermore, the powder metallurgy parking limit block has a density of >6.8 g / cm 3 The roughness of the first inner hole area 101, the second inner hole area 102, and the step slope 103 is not greater than Ra0.8; the roughness of the positioning hole is not greater than Ra1.6.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The production method of the powder metallurgy parking limit block of the present invention effectively overcomes the problems of the prior art in producing the parking limit block of the specific structure of the present invention, which is difficult to process and manufacture, has low production efficiency, and has high comprehensive production cost due to the aforementioned complex structure, high requirements for inner surface finish and angle, etc.

[0034] (2) The production method of the powder metallurgy parking limit block of the present invention can achieve a smooth transition between the first inner hole area, the second inner hole area and the step slope of the parking limit block by matching specific raw materials and combining a specific production process. It can effectively improve the production efficiency while ensuring that the surface roughness of the step slope of the semicircular inner hole of the parking limit block is not greater than Ra0.8 and the angle tolerance is controlled within ±1°. Compared with the existing technology, it effectively increases the number of qualified products produced per unit time, and the production efficiency is improved by more than 50%.

[0035] (3) The method for producing a powder metallurgy parking stop block of the present invention has high precision. The hole tolerance can be controlled below 0.1 mm, the angle tolerance can be controlled below ±1°, and the roundness can be controlled below 0.01 mm, which effectively improves the production yield rate to 99.3%.

[0036] (4) The method for producing a powder metallurgy parking limit block of the present invention has stable performance and controllable quality of the parking limit block. The powder metallurgy parking limit block has stable wear and tear during actual use, effectively eliminates safety hazards, and can meet safety requirements.

[0037] (5) The production method of the powder metallurgy parking limit block of the present invention is simple and efficient. Through compression molding, sintering, machining center drilling, and quenching, a parking limit block that meets the accuracy and angle requirements can be produced. The production process is fast and efficient and can meet the requirements of industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a three-dimensional diagram of the powder metallurgy parking limit block of the present invention;

[0039] Figure 2 A top view of the powder metallurgy parking limit block of the present invention;

[0040] Figure 3 for Figure 2 Sectional view at AA in the figure;

[0041] Figure 4 for Figure 2 The cross-sectional view at BB in FIG.

[0042] In the figure, 10 is a semicircular inner hole, 20 is a positioning wall, 101 is a first inner hole area, 102 is a second inner hole area, 103 is a step slope, 201 is a first positioning hole, and 202 is a second positioning hole. DETAILED DESCRIPTION

[0043] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0044] Example 1

[0045] like Figure 1-4 As shown, a powder metallurgy parking limit block comprises: a semicircular inner hole 10 and a positioning wall 20;

[0046] The semicircular inner hole 10 is in a hollow semicircular arc shape, and an accommodating space is formed in the arc region of the semicircular arc so as to slide relative to the parking shaft and the parking matching piece, thereby realizing parking limit.

[0047] The semicircular inner hole 10 includes: a first inner hole area 101 and a second inner hole area 102 ; the first inner hole area 101 and the second inner hole area 102 are connected by a step transition; the step is a smooth step slope 103 .

[0048] The outer diameter of the first inner hole region 101 is equal to the outer diameter of the second inner hole region 102 .

[0049] The inner diameter of the first inner hole region 101 is greater than the inner diameter of the second inner hole region 102 .

[0050] The ratio of the inner diameters of the first inner hole region 101 and the second inner hole region 102 is 1.05-1.1:1.

[0051] The roughness of the first inner hole area 101, the second inner hole area 102, and the step slope 103 is not greater than Ra0.8.

[0052] A fillet is provided at the connection between the first inner hole region 101 and the step slope 103 to ensure a smooth transition between the first inner hole region 101 and the step slope 103 .

[0053] A fillet is provided at the connection between the second inner hole region 102 and the step slope 103 to ensure a smooth transition between the second inner hole region 102 and the step slope 103 .

[0054] The positioning wall 20 is arranged on the opposite side of the accommodating space of the semicircular inner hole 10 and is integrally formed with the outer wall of the semicircular inner hole 10 to fix the powder metallurgy parking limit block at a predetermined position.

[0055] The positioning wall 20 is provided with two positioning holes: a first positioning hole 201 and a second positioning hole 202 .

[0056] The two positioning holes are arranged in sequence along the direction from the first inner hole area 101 to the second inner hole area 102 .

[0057] The positioning holes are all positioning step holes.

[0058] The roughness of the positioning step hole is not greater than Ra1.6.

[0059] Example 2

[0060] A method for producing a powder metallurgy parking limit block, as follows:

[0061] 1. Ingredients

[0062] Iron powder, copper powder, graphite and lubricant are put into a mixer and mixed evenly to obtain a mixture.

[0063] The lubricant is a conventional lubricant in the field of powder metallurgy. The lubricant used in this embodiment is stearic acid, and the amount of the lubricant added is 0.5wt% of the total mass of the mixture.

[0064] 2. Suppression

[0065] The mixed material is pressed and formed using an upper and lower powder forming die frame to produce a blank.

[0066] The density of the blank is 6.85 g / cm 3 .

[0067] The pressing pressure is 30T, the demoulding pressure is 15T, and the powder addition amount of the mixture is twice the volume of the mold.

[0068] 3. Sintering

[0069] The blank was sintered in a mesh belt sintering furnace at a sintering temperature of 1110° C. for 40 minutes. After the sintering was completed, a sintered part was obtained.

[0070] During sintering, the blank was placed on a flat graphite plate in two layers.

[0071] 4. Drilling

[0072] The sintered part is placed in the machining center, and the positioning holes are drilled using alloy drills and milling cutters.

[0073] For the drilling, the spindle speed of the machining center is 5000 rpm.

[0074] 5. Quenching

[0075] The drilled sintered part was placed in a mesh belt quenching furnace, and quenched and tempered in sequence. Then, it was subjected to vibration grinding, full appearance inspection, and soaked in anti-rust oil to obtain the powder metallurgy parking limit block described in Example 1, with a production yield of 99.3%.

[0076] The quenching temperature is 810°C and the tempering temperature is 180°C.

[0077] The quenching and tempering treatment time is 1 hour.

[0078] The vibration grinding has a power of 3.5 KW and a vibration grinding time of 60 min.

[0079] The powder metallurgy parking limit block contains, by mass%, 0.2% C, 1.0% Cu, and the remainder Fe and unavoidable impurities.

[0080] The powder metallurgy parking limit block has a density of 6.89 g / cm 3 The inner diameter of the first inner hole area 101 is φ18.41, and the inner diameter of the second inner hole area 102 is φ19.91; the roughness of the first inner hole area 101, the second inner hole area 102, and the step slope 103 is Ra0.8, and the roughness of the first positioning hole 201 and the second positioning hole 202 is Ra1.6.

[0081] Example 3

[0082] A method for producing a powder metallurgy parking limit block, as follows:

[0083] 1. Ingredients

[0084] Iron powder, copper powder, graphite and lubricant are put into a mixer and mixed evenly to obtain a mixture.

[0085] The lubricant is a conventional lubricant in the field of powder metallurgy. The lubricant used in this embodiment is zinc stearate, and the amount of the lubricant added is 0.7wt% of the total mass of the mixture.

[0086] 2. Suppression

[0087] The mixed material is pressed and formed using an upper and lower powder forming die frame to produce a blank.

[0088] The density of the blank is 6.90 g / cm 3 .

[0089] The pressing pressure is 31T, the demoulding pressure is 16T, and the powder addition amount of the mixture is 2.1 times of the mold volume.

[0090] 3. Sintering

[0091] The blank was sintered in a mesh belt sintering furnace at a sintering temperature of 1120° C. for 45 minutes. After the sintering was completed, a sintered part was obtained.

[0092] During sintering, the blank was placed on a flat graphite plate in two layers.

[0093] 4. Drilling

[0094] The sintered part is placed in the machining center, and the positioning holes are drilled using alloy drills and milling cutters.

[0095] For the drilling, the spindle speed of the machining center is 5500 rpm.

[0096] 5. Quenching

[0097] The drilled sintered part was placed in a mesh belt quenching furnace, and quenched and tempered in sequence. Then, it was subjected to vibration grinding, full appearance inspection, and soaked in anti-rust oil to obtain the powder metallurgy parking limit block described in Example 1, with a production yield rate of 99.2%.

[0098] The quenching temperature is 820°C and the tempering temperature is 185°C.

[0099] The time for the quenching and tempering treatment is 1.1 h.

[0100] The vibration grinding has a power of 4KW and a vibration grinding time of 65min.

[0101] The powder metallurgy parking limit block contains, by mass%, 0.6% C, 3.0% Cu, and the remainder Fe and unavoidable impurities.

[0102] The powder metallurgy parking limit block has a density of 6.91 g / cm 3 The inner diameter of the first inner hole area 101 is φ18.50, the inner diameter of the second inner hole area 102 is φ19.93, the roughness of the first inner hole area 101, the second inner hole area 102, and the step slope 103 is Ra0.8, and the roughness of the first positioning hole 201 and the second positioning hole 202 is Ra1.6.

[0103] Example 4

[0104] A method for producing a powder metallurgy parking limit block, as follows:

[0105] 1. Ingredients

[0106] Iron powder, copper powder, graphite and lubricant are put into a mixer and mixed evenly to obtain a mixture.

[0107] The lubricant is a conventional lubricant in the field of powder metallurgy. The lubricant used in this embodiment is stearic acid amide, and the added amount of the lubricant is 0.9wt% of the total mass of the mixture.

[0108] 2. Suppression

[0109] The mixed material is pressed and formed using an upper and lower powder forming die frame to produce a blank.

[0110] The density of the blank is 6.95 g / cm 3 .

[0111] The pressing pressure is 32T, the demoulding pressure is 17T, and the powder addition amount of the mixture is 2.2 times of the mold volume.

[0112] 3. Sintering

[0113] The blank was sintered in a mesh belt sintering furnace at a sintering temperature of 1130° C. for 50 minutes. After the sintering was completed, a sintered part was obtained.

[0114] During sintering, the blank was placed on a flat graphite plate in two layers.

[0115] 4. Drilling

[0116] The sintered part is placed in the machining center, and the positioning holes are drilled using alloy drills and milling cutters.

[0117] For the drilling, the spindle speed of the machining center is 6000 rpm.

[0118] 5. Quenching

[0119] The drilled sintered part was placed in a mesh belt quenching furnace, and quenched and tempered in sequence. Then, it was subjected to vibration grinding, full appearance inspection, and rust-proof oil immersion to obtain the powder metallurgy parking limit block described in Example 1, with a production yield of 99.0%.

[0120] The quenching temperature is 830°C and the tempering temperature is 190°C.

[0121] The time for the quenching and tempering treatment is 1.2 h.

[0122] The vibration grinding has a power of 5KW and a vibration grinding time of 70min.

[0123] The powder metallurgy parking limit block contains, by mass%, 1.0% C, 5.0% Cu, and the remainder Fe and unavoidable impurities.

[0124] The powder metallurgy parking limit block has a density of 6.98g / cm 3 The inner diameter of the first inner hole area 101 is φ18.48, the inner diameter of the second inner hole area 102 is φ19.97, the roughness of the first inner hole area 101, the second inner hole area 102, and the step slope 103 is Ra0.8, and the roughness of the first positioning hole 201 and the second positioning hole 202 is Ra1.6.

[0125] Example 5

[0126] A method for producing a powder metallurgy parking limit block, as follows:

[0127] 1. Ingredients

[0128] Iron powder, copper powder, graphite, lubricant and reinforcing agent are put into a mixer and mixed evenly to obtain a mixture.

[0129] The lubricant is a conventional lubricant in the field of powder metallurgy. The lubricant used in this embodiment is stearic acid, and the amount of the lubricant added is 0.5wt% of the total mass of the mixture.

[0130] The production method of the reinforcing agent comprises the following steps: putting a predetermined amount of carbon fiber, polyethylene isobutyl ether, sodium N-hydroxymethylglycinate, zinc stearate, and coupling agent KH-550 into a ball mill, controlling the ball-to-material ratio to be 12:1, the ball milling speed to be 650 rpm, and the ball milling time to be 30 minutes to obtain a ball milled product; placing the ball milled product in a nitrogen atmosphere at 40° C. 60The ball-milled material was irradiated with a Co radiation source, and the irradiation dosage was controlled to be 100 KGy. After the irradiation treatment, the pressure was increased to 12 MPa at a pressure rate of 3 MPa / min and the pressure was maintained for 20 min. Then, the material was allowed to stand at 80°C for 1 h in a vacuum environment of 0.08 MPa to obtain a reinforcing agent.

[0131] Among them, the weight ratio of carbon fiber, polyethylene isobutyl ether, sodium N-hydroxymethylglycinate, zinc stearate and coupling agent KH-550 is 30:10:2:12:0.2.

[0132] The length of the carbon fiber is 8 μm.

[0133] The amount of the reinforcing agent added is 3wt% of the total mass of the mixture.

[0134] 2. Suppression

[0135] The mixed material is pressed and formed using an upper and lower powder forming die frame to produce a blank.

[0136] The density of the blank is 6.85 g / cm 3 .

[0137] The pressing pressure is 30T, the demoulding pressure is 15T, and the powder addition amount of the mixture is twice the volume of the mold.

[0138] 3. Sintering

[0139] Under a pressure of 20 MPa, a high-energy pulse current was used to heat the blank to 800°C and keep it warm for 20 minutes; then the temperature was raised to 950°C and kept warm for 10 minutes; then the temperature was raised to 1120°C at a heating rate of 20°C / min and kept warm for 15 minutes to obtain a sintered part.

[0140] 4. Drilling

[0141] The sintered part is placed in the machining center, and the positioning holes are drilled using alloy drills and milling cutters.

[0142] For the drilling, the spindle speed of the machining center is 6000 rpm.

[0143] 5. Quenching

[0144] The drilled sintered part is placed in a mesh belt quenching furnace, and quenched and tempered in sequence. Then, it is subjected to vibration grinding, full appearance inspection, and immersion in anti-rust oil to obtain the powder metallurgy parking limit block described in Example 1, and the production yield rate reaches 99.5%.

[0145] The quenching temperature is 820°C and the tempering temperature is 180°C.

[0146] The quenching and tempering treatment time is 1 hour.

[0147] The vibration grinding has a power of 5KW and a vibration grinding time of 60min.

[0148] The powder metallurgy parking limit block contains, by mass%, 1.0% C, 3.0% Cu, and the remainder Fe and unavoidable impurities.

[0149] The powder metallurgy parking limit block has a density of 6.86 g / cm 3 The inner diameter of the first inner hole area 101 is φ18.40, the inner diameter of the second inner hole area 102 is φ19.90, the roughness of the first inner hole area 101, the second inner hole area 102, and the step slope 103 is Ra0.4, and the roughness of the first positioning hole 201 and the second positioning hole 202 is Ra1.6.

[0150] Unless otherwise specified, all percentages used in the present invention are by mass.

[0151] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for producing a powder metallurgy parking limit block, characterized in that: The production method includes: batching, pressing, sintering, drilling, and quenching; The ingredients are: iron powder, copper powder, graphite, lubricant, and reinforcing agent are put into a mixer and mixed evenly to obtain a mixture; The lubricant is stearic acid, and the amount of the lubricant added is 0.5wt% of the total mass of the mixture; The production method of the reinforcing agent comprises the following steps: putting a predetermined amount of carbon fiber, polyethylene isobutyl ether, sodium N-hydroxymethylglycinate, zinc stearate, and coupling agent KH-550 into a ball mill, controlling the ball-to-material ratio to be 12:1, the ball milling speed to be 650 rpm, and the ball milling time to be 30 minutes, to obtain a ball milled product; placing the ball milled product in a nitrogen atmosphere, irradiating the ball milled product with a 60Co radiation source at 40° C., and controlling the irradiation dosage to be 100 KGy; after the irradiation treatment, pressurizing the product to 12 MPa at a pressurizing rate of 3 MPa / min, and maintaining the pressure for 20 minutes; and then standing the product at 80° C. for 1 hour in a vacuum environment of 0.08 MPa, to obtain the reinforcing agent; In the production method of the reinforcing agent, the weight ratio of carbon fiber, polyethylene isobutyl ether, sodium N-hydroxymethylglycinate, zinc stearate, and coupling agent KH-550 is 30:10:2:12:0.2; The length of the carbon fiber is 8 μm; The amount of the reinforcing agent added is 3wt% of the total mass of the mixture; The pressing process is to press the mixed material into a blank; the density of the blank is 6.85 g / cm 3 ; The pressing pressure is 30T, the demoulding pressure is 15T, and the powder addition amount of the mixture is 2 times the volume of the mold; The sintering process is as follows: the blank is heated to 800°C under a pressure of 20 MPa and kept at this temperature for 20 minutes; then the blank is heated to 950°C and kept at this temperature for 10 minutes; then the blank is heated to 1120°C at a heating rate of 20°C / min and kept at this temperature for 15 minutes to obtain a sintered part; For the drilling, the spindle speed of the machining center is 6000 rpm; The quenching process is to sequentially quench and temper the sintered part after drilling, and then vibrate grind, inspect the appearance, and soak it in anti-rust oil to obtain a powder metallurgy parking limit block; The quenching temperature is 820°C and the tempering temperature is 180°C; The quenching and tempering treatment time is 1h; The vibration grinding has a power of 5KW and a vibration grinding time of 60min; The powder metallurgy parking limit block contains, by mass%, 1.0% C, 3.0% Cu, and the remainder Fe and unavoidable impurities.

Citation Information

Patent Citations

  • Manufacture method for automobile 5DYA limited block

    CN102198508A

  • Gear component for adjusting automobile seat armrest

    CN106335415A

  • Multi-mold-box parking braking mechanism

    CN214146556U