Rosin-based polyether polyol and preparation method and application thereof

Through the polymerization of rosin glyceride and polyols under the action of a catalyst, the problem of harsh synthesis conditions of existing rosin-modified polyols is solved, and rosin-based polyether polyols with heat resistance and high mechanical strength are prepared, achieving a green and environmentally friendly The low-cost preparation of polyurethane foam materials replaces petroleum resources and improves the thermal conductivity and activity of the material.

CN116178696BActive Publication Date: 2024-10-15SHANDONG INOV NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211594231.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-10-15
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

The synthesis conditions of existing rosin-modified polyols are harsh and the steps are numerous, making it difficult to prepare them industrially on a large scale at low cost. In addition, the raw materials of rigid polyurethane foams are mainly derived from petroleum resources, and they are faced with price, resource and environmental pressures.

Method used

Rosin glyceryl ester and polyol are polymerized with alkylene oxide under the action of a catalyst to prepare rosin-based polyether polyol. Rosin glyceryl ester is prepared through esterification reaction, and the temperature is raised for polymerization in a nitrogen atmosphere, and then alkylene oxide is added dropwise. Perform chain extension and end-capping synthesis, and finally perform nitrogen bubbling to remove residual small molecules.

Benefits of technology

The prepared rosin-based polyether polyol has good heat resistance, high mechanical strength and good water resistance, and is a green and environmentally friendly material. It can replace petrochemical products and has low cost. It is suitable for the preparation of rigid polyurethane foam and improves the efficiency of the production process. Thermal conductivity and activity of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 511131DEST_PATH_IMAGE003
    Figure 511131DEST_PATH_IMAGE003
  • Figure 62832DEST_PATH_IMAGE001
    Figure 62832DEST_PATH_IMAGE001
  • Figure DEST_PATH_IMAGE002
    Figure DEST_PATH_IMAGE002
Patent Text Reader

Abstract

The invention belongs to the technical field of polyether polyol preparation, and specifically relates to rosin-based polyether polyol and a preparation method and application thereof. The rosin-based polyether polyol is obtained by polymerizing rosin glycerol ester and polyol as mixed initiators with alkylene oxide under the action of a catalyst; wherein the rosin glycerol ester is prepared by esterification reaction of rosin and glycerol in a molar ratio of (1-6):3. The polyether polyol of the invention has good heat resistance, high mechanical strength, good water resistance and is green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyether polyol preparation, and in particular relates to rosin-based polyether polyol and a preparation method and application thereof. Background Art

[0002] Rigid foam polyether polyol is the main upstream raw material of current polyurethane insulation products. It is a polyether polyol with sufficient crosslinking degree and rigidity, as well as high functionality, high hydroxyl value and low molecular weight. Its functionality is generally 3~8, and its hydroxyl value is 300~700mgKOH / g. Rigid foam polyether polyol reacts with polyisocyanate after mixing with foaming agent and catalyst to form a foam with a crosslinked network structure. The foam products formed have high hardness, high compression strength, good dimensional stability and temperature resistance, and are often used in home appliance insulation, industrial insulation, building energy conservation and other fields. Polyether polyols with different compound structures are used in rigid polyurethane foam plastics to obtain various performance properties. Chinese patent CN101045785A [2007.10.03] discloses a rosin-modified polyether polyol using hydroxymethyl rosin, a catalyst, a small molecule alcohol and ethylene oxide / propylene oxide as raw materials and a preparation method thereof, which can be used for rigid polyurethane foam plastics; Chinese patent CN107177314B [2018.04.17] uses rosin, a diene adduct, a catalyst and a polyol / sorbitol modifier as raw materials to prepare a rosin diene adduct polyol resin, which can be used to prepare an aqueous environmentally friendly tackifying emulsion.

[0003] As mentioned above, rosin-modified polyols obtained by different compound structures and preparation methods can be used to prepare polyurethane materials of different forms to obtain different performance properties. The synthesis of rosin-modified polyols in the prior art is either harsh or has many steps, which makes it difficult to prepare them on a large scale at low cost in industry. The development process is simple, and the synthesis route with lower energy consumption can save the utilization cost of rosin, which is conducive to the promotion and use of rosin-modified polyols and better improves the added value of rosin. In addition, the raw materials used in the production of rigid polyurethane foams are all taken from petroleum resources, and the development and utilization of petroleum resources are also faced with price, resource and environmental pressure. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a rosin-based polyether polyol with good heat resistance, high mechanical strength, good water resistance and environmental protection. The present invention also provides a scientific and reasonable preparation method. The rosin-based polyether polyol prepared by the present invention can be used to prepare rigid polyurethane foam.

[0005] The rosin-based polyether polyol of the present invention is obtained by polymerizing rosin glycerol ester and polyol as mixed initiators with alkylene oxide under the action of a catalyst;

[0006] Among them, rosin glycerol ester is prepared by esterification reaction of rosin and glycerol in a molar ratio of (1~6):3.

[0007] The mass percentage of rosin glycerol ester in the mixed initiator is (20~62)%.

[0008] The mass percentage of polyol in the mixed initiator is (38~80)%.

[0009] The polyol is one or more of sucrose, sorbitol, 1,4-butanediol, diethanolamine, diethylene glycol, tricyclodecane dimethanol, neopentyl glycol and 1,4-cyclohexanedimethanol.

[0010] The catalyst is a basic catalyst or a mixture of a basic catalyst and one or more of triethylamine, N,N-dimethylbenzylamine and dimethylcyclohexylamine.

[0011] The alkaline catalyst is one or more of KOH, DMA and potassium methoxide.

[0012] The alkylene oxide is one or more of propylene oxide, ethylene oxide and butylene oxide.

[0013] The preparation method of rosin glycerol ester is as follows: add rosin, glycerol and zinc oxide into a reaction kettle, heat up to 200-220°C, start stirring after the rosin is melted, and heat up from 220°C to 270°C within 20-40min; continue heating and control the temperature not higher than 290°C, react for 2-2.5h; continue heating until the temperature is higher than 290°C to remove volatiles, and obtain rosin glycerol ester.

[0014] After the temperature reaches 270℃, the esterification reaction begins. The boiling point of glycerol is 290℃. During the esterification reaction, it is important to control the temperature so that it does not reach or exceed 290℃, so as to avoid glycerol evaporation loss, which will lead to insufficient glycerol in the esterification stage. The esterification reaction mainly takes place in the first hour or so, and then the reaction gradually slows down. The purpose of continuing to heat up is to make the reaction more complete. When it reaches 290℃, continue to heat to remove excess water and volatiles such as glycerol, and finally obtain rosin glycerol ester.

[0015] The preparation method of the rosin-based polyether polyol of the present invention comprises the following steps:

[0016] (1) Add rosin glycerol ester, polyol and catalyst into the reactor, heat it to 105-115°C under nitrogen atmosphere, pressurize it with nitrogen to 0.2-0.3 MPa and react for 2-3 hours;

[0017] (2) Cooling to 80-85°C, evacuating, and then dropping epoxy olefin compounds to carry out polyether chain extension. After the feeding is completed, the internal pressure reaction is continued for 1-2 hours to obtain an intermediate rosin-based polyether polyol;

[0018] (3) The intermediate rosin-based polyether polyol is heated to 125-135°C, and alkylene oxide is added dropwise for end-capping synthesis. After the feeding is completed, the internal pressure reaction is continued for 2-3 hours to obtain a rosin-based polyether polyol crude polymer, which is pressurized to 0.2-0.3 MPa with nitrogen filling and the pressure does not decrease any more;

[0019] (4) The crude polymer of rosin-based polyether polyol is cooled to 95-105°C and then nitrogen is bubbled to remove residual small molecules. After bubbling for 1-2 hours, the crude polymer is cooled to 75-80°C and then discharged to obtain rosin-based polyether polyol.

[0020] The application of the rosin-based polyether polyol of the present invention is suitable for the preparation of rigid polyurethane foam.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The rosin used in the present invention is a natural resin, which can be used as a renewable green environmentally friendly material to replace petrochemical products, and has the advantages of low cost and good environmental protection when used to prepare polymer materials;

[0023] 2. The rosin-based polyether polyol prepared by the present invention has better mechanical strength, activity, pentane miscibility and thermal conductivity than other polyether polyols when used for polyurethane synthesis by introducing the ternary phenanthrene ring structure in rosin. DETAILED DESCRIPTION

[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.

[0025] Unless otherwise specified, all raw materials used in the examples are commercially available.

[0026] Example 1

[0027] The preparation method of rosin glycerol ester of the present invention comprises the following steps: adding 302g of rosin, 276g of glycerol and 3g of zinc oxide into a reaction kettle, heating the kettle to 210°C, stirring the kettle after the rosin is melted, and heating the kettle from 220°C to 270°C within 30min; continuously heating the kettle and controlling the temperature not to be higher than 290°C, reacting the kettle for 2h; and continuing heating the kettle until the temperature is higher than 290°C to remove volatiles, thereby obtaining rosin glycerol ester.

[0028] The preparation method of the rosin-based polyether polyol of the present invention mainly comprises the following steps:

[0029] Add 500g of rosin glycerol ester, 150g of sucrose, 115g of diethanolamine, 20g of diethylene glycol, 40g of 1,4-cyclohexanedimethanol, 5g of KOH and 9g of triethylamine catalyst into the reactor, close the reactor and test for leakage and replace, then heat to 105-115°C under nitrogen atmosphere, after heating, pressurize with nitrogen to 0.2-0.3MPa, and react for 2-3h;

[0030] The temperature was lowered to 80-85°C, and after vacuuming to -0.09 MPa, 220 g of ethylene oxide was added dropwise to extend the polyether chain. After the feeding was completed, the internal pressure reaction was continued for 1-2 hours to obtain an intermediate polyether polyol.

[0031] The intermediate polyether polyol was heated to 125-135°C, and 147 g of propylene oxide was continuously added dropwise for end-capping synthesis. After the feeding was completed, the temperature was kept high, and the internal pressure reaction was continued for 2-3 hours. The reactor was pressurized to 0.25 MPa with nitrogen filling, and the pressure in the reactor did not decrease any more.

[0032] After cooling to 95-105°C, nitrogen bubbling is performed to remove residual small molecular substances in the product. After bubbling for 1-2 hours, the temperature is lowered to 80°C and the polyether polyol A is obtained by discharging.

[0033] Example 2

[0034] The preparation method of the rosin glycerol ester of the present invention is the same as that of Example 1.

[0035] The preparation method of the rosin-based polyether polyol of the present invention mainly comprises the following steps:

[0036] Add 365g of rosin glycerol ester, 180g of sucrose, 85g of diethanolamine, 20g of diethylene glycol, 40g of neopentyl glycol, 4g of DMA and 5g of N,N-dimethylbenzylamine catalyst into the reactor, close the reactor and test for leakage and replace, then heat to 105-115°C under nitrogen atmosphere, pressurize with nitrogen to 0.2-0.3MPa after heating, and react for 2-3h;

[0037] The temperature was lowered to 80-85°C, and after vacuuming to -0.09 MPa, 396 g of ethylene oxide was added dropwise to extend the polyether chain. After the feeding was completed, the internal pressure reaction was continued for 1-2 hours to obtain an intermediate polyether polyol.

[0038] The intermediate polyether polyol was heated to 125-135°C, and 291 g of propylene oxide was continuously added dropwise for end-capping synthesis. After the feeding was completed, the temperature was kept high and the internal pressure was continued for 2-3 hours. The pressure was increased to 0.25 MPa with nitrogen filling and the pressure in the kettle did not decrease any more.

[0039] After cooling to 95-105°C, nitrogen bubbling is performed to remove residual small molecular substances in the product. After bubbling for 1-2 hours, the temperature is lowered to 80°C and the polyether polyol B is obtained by discharging.

[0040] Example 3

[0041] The preparation method of the rosin glycerol ester of the present invention is the same as that of Example 1.

[0042] The preparation method of the rosin-based polyether polyol of the present invention mainly comprises the following steps:

[0043] Add 306g of rosin glycerol ester, 200g of sucrose, 52.6g of diethanolamine, 46g of tricyclodecane dimethanol, 3g of potassium methoxide, 4g of N,N-dimethylbenzylamine and 4g of dimethylcyclohexylamine catalyst into the reactor, close the reactor and test for leakage and replace, then heat to 105-115°C under nitrogen atmosphere, pressurize with nitrogen to 0.2-0.3MPa after heating, and react for 2-3h;

[0044] The temperature was lowered to 80-85°C, and after vacuuming to -0.09 MPa, 228 g of ethylene oxide was added dropwise to extend the polyether chain. After the feeding was completed, the internal pressure reaction was continued for 1-2 hours to obtain an intermediate polyether polyol.

[0045] The intermediate polyether polyol was heated to 125-135°C, and 58 g of propylene oxide was continuously added dropwise for end-capping synthesis. After the feeding was completed, the temperature was kept high and the internal pressure was continued for 2-3 hours. The pressure was increased to 0.25 MPa with nitrogen filling and the pressure in the kettle did not decrease any more.

[0046] After cooling to 95-105°C, nitrogen bubbling is performed to remove residual small molecular substances in the product. After bubbling for 1-2 hours, the temperature is lowered to 80°C and the material is discharged to obtain polyether polyol C.

[0047] Example 4

[0048] The preparation method of the rosin glycerol ester of the present invention is the same as that of Example 1.

[0049] The preparation method of the rosin-based polyether polyol of the present invention mainly comprises the following steps:

[0050] Add 200g of rosin glycerol ester, 230g of sucrose, 15g of solid sorbitol, 65g of diethanolamine, 25g of 1,4-butanediol, 4g of KOH, 4g of N,N-dimethylbenzylamine and 4g of dimethylcyclohexylamine catalyst into the reactor, close the reactor and test for leakage and replace, then heat to 105-115°C under nitrogen atmosphere, pressurize with nitrogen to 0.2-0.3MPa after heating, and react for 2-3h;

[0051] The temperature was lowered to 80-85°C, and after vacuuming to -0.09 MPa, 230 g of ethylene oxide was added dropwise to extend the polyether chain. After the feeding was completed, the internal pressure reaction was continued for 1-2 hours to obtain an intermediate polyether polyol.

[0052] The intermediate polyether polyol was heated to 125-135°C, and 63 g of propylene oxide was continuously added dropwise for end-capping synthesis. After the feeding was completed, the temperature was kept high and the internal pressure was continued for 2-3 hours. The pressure was increased to 0.25 MPa with nitrogen filling and the pressure in the kettle did not decrease any more.

[0053] After cooling to 95-105°C, nitrogen bubbling was performed to remove residual small molecular substances in the product. After bubbling for 1-2 hours, the temperature was lowered to 80°C and the polyether polyol D was obtained by discharging.

[0054] Comparative Example 1

[0055] 325 g of sucrose, 50 g of solid sorbitol, 80 g of diethylene glycol, 255 g of palm oil and 12 g of fatty amine catalyst were added to the reactor. After the reactor was closed for leak testing and replacement, the temperature was raised to 105°C under negative pressure. At the same time, the nitrogen atmosphere pressure in the reactor was maintained at 0.13±0.02 MPa. 787 g of propylene oxide was dripped into the reactor. After the dripping of propylene oxide was completed, the reaction was continued for 3 hours while keeping the temperature warm until the pressure in the reactor no longer decreased. After bubbling and stripping of monomers for 2 hours, the temperature was lowered to 80°C and the material was discharged to obtain polyether polyol E.

[0056] Comparative Example 2

[0057] 325g of sucrose, 165g of diethylene glycol and 11.4g of chromium acetylacetonate catalyst were added to the reactor. After the reactor was closed for leak testing and replacement, the temperature was raised to 105°C under negative pressure. At the same time, the nitrogen atmosphere pressure in the reactor was maintained at 0.13±0.02MPa. 913g of propylene oxide was dripped into the reactor. After the dripping of propylene oxide was completed, the temperature was kept warm and the reaction was continued for 3h until the pressure in the reactor no longer decreased. After bubbling and stripping of monomers for 2h, the temperature was lowered to 80°C and the material was discharged to obtain polyether polyol F.

[0058] Performance Test:

[0059] The polyether polyols obtained in Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests according to the following standards. The results are shown in Table 1.

[0060] Hydroxyl value: GB / T12008.3-1989 "Determination of hydroxyl value in polyether polyols";

[0061] Viscosity: GB / T12008.7-2010 "Plastic polyether polyols Part 7: Determination of viscosity".

[0062] Table 1 Performance index test table of Examples 1 to 4 and Comparative Examples 1 to 2

[0063]

[0064] The polyether polyols obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were formulated according to the formula shown in Table 2, wherein PC8 is a gel catalyst, MAYCAT PC8 from Jiangsu Meside Chemical Co., Ltd.; 8815 is a uniform foaming agent, M-8815 from Jiangsu Meside Chemical Co., Ltd.;

[0065] Preparation method of polyurethane foam sample: PM200, Wanhua Chemical Group Co., Ltd. is selected as the black material, and the white material is prepared as the combined material according to Table 2. The black material and the white material are evenly mixed to obtain the polyurethane foam sample.

[0066] Table 2 Rigid polyurethane foam formulations of Examples 1 to 4 and Comparative Examples 1 to 2

[0067]

[0068] The obtained polyurethane foam samples were tested for performance according to the following standards or methods. The results are shown in Table 3.

[0069] Strength: Tested in accordance with GB / T8813-2020 "Determination of compression properties of rigid foam plastics";

[0070] Activity: The time from the time the black and white materials are mixed and stirred to the time they start to hair and draw. The shorter the time, the higher the activity.

[0071] Test method for the miscibility of n-pentane and cyclopentane: at 25°C, gradually add cyclopentane or n-pentane to 100 parts by mass of polyether polyol, mix evenly, until the polyether polyol changes from clear to turbid, and record the mass fraction of pentane used at the critical point of change. According to GB / T10801.1-2002 standard, the thermal conductivity of polyurethane rigid foam is required to be ≤0.024W / (m·K).

[0072] Table 3 Performance test results of polyurethane foam products prepared from products of Examples 1 to 4 and Comparative Examples 1 to 2

[0073]

[0074] From the data in Table 3, the present invention meets the thermal conductivity requirements of polyurethane rigid foam in GB / T10801.1-2002 standard; by comparing Examples 1 to 4 with Comparative Examples 1 to 2, it can be seen that the rigid polyurethane foam prepared by the polyether polyol of the present invention has high strength and activity; good miscibility with pentane, and improved miscibility with n-pentane and cyclopentane; and significantly improved thermal conductivity.

Claims

1. A rosin-based polyether polyol, characterized in that: It is obtained by polymerizing rosin glycerol ester and polyol as mixed initiators with alkylene oxide under the action of catalyst. Wherein, rosin glycerol ester is prepared by esterification reaction of rosin and glycerol in a molar ratio of (1-6):3; The polyol is one or more of sucrose, sorbitol, 1,4-butanediol, diethanolamine, diethylene glycol, tricyclodecane dimethanol, neopentyl glycol and 1,4-cyclohexanedimethanol.

2. The rosin-based polyether polyol according to claim 1, characterized in that The mass percentage of rosin glycerol ester in the mixed initiator is (20~62)%.

3. The rosin-based polyether polyol according to claim 1, characterized in that The mass percentage of polyol in the mixed initiator is (38~80)%.

4. The rosin-based polyether polyol according to claim 1, characterized in that The catalyst is a basic catalyst or a mixture of a basic catalyst and one or more of triethylamine, N,N-dimethylbenzylamine and dimethylcyclohexylamine.

5. The rosin-based polyether polyol according to claim 4, characterized in that The alkaline catalyst is one or more of KOH, DMA and potassium methoxide.

6. The rosin-based polyether polyol according to claim 1, characterized in that The alkylene oxide is one or more of propylene oxide, ethylene oxide and butylene oxide.

7. The rosin-based polyether polyol according to claim 1, characterized in that The preparation method of rosin glycerol ester is as follows: add rosin, glycerol and zinc oxide into a reaction kettle, heat up to 200-220°C, start stirring after the rosin is melted, and heat up from 220°C to 270°C within 20-40min; continue heating and control the temperature not higher than 290°C, react for 2-2.5h; continue heating until the temperature is higher than 290°C to remove volatiles, and obtain rosin glycerol ester.

8. A method for preparing a rosin-based polyether polyol according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Add rosin glycerol ester, polyol and catalyst into the reactor, heat it to 105-115°C under nitrogen atmosphere, pressurize it with nitrogen to 0.2-0.3 MPa and react for 2-3 hours; (2) Cooling to 80-85°C, evacuating, and then dropping alkylene oxide to carry out polyether chain extension. After the feeding is completed, the internal pressure reaction is continued for 1-2 hours to obtain an intermediate rosin-based polyether polyol; (3) The intermediate rosin-based polyether polyol is heated to 125-135°C, and alkylene oxide is added dropwise for end-capping synthesis. After the feeding is completed, the internal pressure reaction is continued for 2-3 hours to obtain a rosin-based polyether polyol crude polymer, which is pressurized to 0.2-0.3 MPa with nitrogen filling and the pressure does not decrease any more; (4) The crude polymer of rosin-based polyether polyol is cooled to 95-105°C and then nitrogen is bubbled to remove residual small molecules. After bubbling for 1-2 hours, the crude polymer is cooled to 75-80°C and then discharged to obtain rosin-based polyether polyol.

9. Use of the rosin-based polyether polyol according to any one of claims 1 to 7, characterized in that: Suitable for the preparation of rigid polyurethane foam.