A molybdenum-lanthanum oxide-yttrium oxide alloy weight, preparation method and application
By using molybdenum-lanthanum oxide-yttrium oxide alloy materials, the process flow is simplified, and the problems of short service life and high cost of existing molybdenum weights in high-temperature environments are solved, and a high-density, uniform grain weight weight is achieved to meet the needs of The demand for stable growth of monocrystalline silicon crystal growth furnaces has increased.
Patent Information
- Application Number
- CN202310043355.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-29
AI Technical Summary
Existing molybdenum weights have a short service life in high-temperature environments, high costs, complex processes, and low material utilization, making it difficult to meet the stable straightening requirements of single-crystal silicon growth furnaces.
Using molybdenum-lanthanum oxide-yttrium oxide alloy material, by mixing molybdenum powder, lanthanum oxide powder and yttrium oxide powder, cold isostatic pressing and multi-stage sintering treatment are performed to form a high-density, uniform grain weight to avoid forging work. order, simplifying the process flow.
A molybdenum-lanthanum oxide-yttrium oxide alloy hammer with a service life of more than one year in a high temperature environment of 1300°C has been achieved, which reduces material costs, simplifies the manufacturing process, and improves material density and tensile properties.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder metallurgy, and relates to a process for preparing a molybdenum weight, and in particular to a molybdenum-lanthanum oxide-yttrium oxide alloy weight, a preparation method and an application thereof. The prepared product can be used as a weight in a single crystal silicon growth furnace. Background Art
[0002] Molybdenum weights are used in single crystal silicon growth furnaces and are hung at the lower end of the suspension rope. They play a role in stabilizing and straightening the weight during the pulling process. The lower end of the molybdenum weight works in the high temperature area of 1300℃ for a long time, which is difficult for materials with low melting points. Therefore, molybdenum materials with high melting points have become the preferred material for weights.
[0003] At present, the existing weight structures are all made of molybdenum material as a whole. Generally, molybdenum powder alloy is sintered into a molybdenum alloy rod, and then cut and forged into a molybdenum alloy weight. Sintered pure molybdenum material is brittle and has low tensile strength. It is easy to be broken during use and cannot meet the requirements well. Although the pure molybdenum material after forging hot processing can have good strength and elongation, the weight is generally large in size, with many diameter changes, high forging process cost, low material utilization rate and low yield rate. Limited by the physical properties of molybdenum material, the weight of molybdenum material is expensive and has high overall cost. Therefore, it is urgent to develop a molybdenum weight with simple manufacturing process, long service life and low manufacturing cost. Summary of the invention
[0004] In view of the above-mentioned defects or deficiencies in the prior art, the present application aims to provide a molybdenum-lanthanum oxide-yttrium oxide alloy weight with a simple manufacturing process, low manufacturing cost and long service life, a preparation method and application.
[0005] One of the purposes of the present invention is to provide a molybdenum-lanthanum oxide-yttrium oxide alloy weight, the weight comprising the following raw materials in percentage by weight: 0.8% to 5% of lanthanum oxide powder, 0.3% to 0.8% of yttrium oxide powder, and the balance being molybdenum powder;
[0006] The average particle size of the molybdenum powder is 3.0-4.0 μm; the particle sizes of the lanthanum oxide powder and the yttrium oxide powder are independently 0.2-2 μm, and the molybdenum powder, lanthanum oxide powder and yttrium oxide powder do not contain single particles with a particle size of ≥20 μm.
[0007] Preferably, the average particle size of the molybdenum powder is 3.5 μm.
[0008] The second object of the present invention is to provide a method for preparing a molybdenum-lanthanum oxide-yttrium oxide alloy weight, the preparation method comprising:
[0009] The raw materials are mixed, pressed and sintered to obtain a sintered compact.
[0010] Preferably, the raw materials are mixed for 20 to 40 hours.
[0011] Preferably, the press forming satisfies at least one of the following process parameters:
[0012] (a) Pressing molding adopts cold isostatic pressing;
[0013] (b) cold isostatic pressing at a pressure of 190 to 230 MPa; and
[0014] (c) The holding time is 10 to 30 minutes.
[0015] Preferably, the green compact obtained by compression molding is vacuum-sealed and stored for later use.
[0016] Preferably, the method further comprises the steps of shaping the pressed product and then sintering it.
[0017] Preferably, the shaping step comprises: shaping the pressed green sheet to obtain a shaped green sheet in an environment with a humidity of ≤20%.
[0018] Preferably, the shaped blank is vacuum-sealed and stored for future use.
[0019] Preferably, the sintering step includes a first sintering stage, a second sintering stage and a third sintering stage. The first sintering stage is to increase the temperature to a first insulation temperature and then keep the temperature for 1 to 4 hours, and the first insulation temperature is 180 to 250°C.
[0020] The second sintering stage is to increase the temperature from the first insulation temperature to the second insulation temperature, and then keep it for 1 to 4 hours. The second insulation temperature is 1300 to 1500°C.
[0021] The third sintering stage is to increase the temperature from the second insulation temperature to the sintering temperature and then keep it for 4 to 8 hours. The sintering temperature is 1950 to 2200°C.
[0022] Preferably, the heating rates of the first sintering stage, the second sintering stage and the third sintering stage are independently 50-100°C / h;
[0023] Preferably, the sintering step is carried out under vacuum or a reducing atmosphere, preferably a hydrogen atmosphere;
[0024] Preferably, the hydrogen flow rate is 2 to 15 m 3 / h.
[0025] Preferably, the preparation method further comprises a step of machining after sintering.
[0026] Preferably, the remaining amount of the sintered green body compared to the finished product made by heavy hammer is 1.5-2 mm on one side.
[0027] The third object of the present invention is to provide a molybdenum-lanthanum oxide-yttrium oxide alloy weight for use in a single crystal silicon growth furnace.
[0028] Preferably, the molybdenum-lanthanum oxide-yttrium oxide alloy weight has a service life of more than 1 year in a high temperature environment exceeding 1300°C.
[0029] The beneficial effects of the present invention include:
[0030] The present invention uses 0.8% to 5% of lanthanum oxide powder, 0.3% to 0.8% of yttrium oxide powder and molybdenum powder, the average particle size of the molybdenum powder is 3.0 to 4.0 μm; the particle sizes of the lanthanum oxide powder and yttrium oxide powder are independently 0.2 to 2 μm, and the molybdenum powder, lanthanum oxide powder and yttrium oxide powder do not have single particles with a particle size of ≥20 μm. The purity of the weight is more than 99.95%, and the relative density reaches more than 97.5%. The grains of the weight are uniform and fine, and the average grain size is no more than 26 μm. In a high temperature environment of 1300°C, the service life is more than 1 year. DETAILED DESCRIPTION
[0031] In the following description, certain specific details are included to provide a comprehensive understanding of each disclosed embodiment. However, one skilled in the relevant art will recognize that the embodiments can be implemented without one or more of these specific details, but with other methods, components, materials, etc.
[0032] Unless otherwise required in this application, throughout the specification and the claims that follow, the words "including" and "comprising" should be interpreted in an open, inclusive sense, ie, "including, but not limited to."
[0033] References to "one embodiment" or "an embodiment" or "a preferred embodiment" or "certain embodiments" throughout this specification mean that the specific referenced elements, structures or features described in connection with the embodiment are included in at least one embodiment. Therefore, the phrases "in one embodiment" or "in an embodiment" or "in a preferred embodiment" or "in certain embodiments" appearing in different places throughout the specification do not necessarily all refer to the same embodiment. In addition, the specific elements, structures or features may be combined in any appropriate manner in one or more embodiments.
[0034] According to a first aspect of the present invention, a molybdenum-lanthanum oxide-yttrium oxide alloy weight is provided, characterized in that the weight comprises the following raw materials in weight percentage: 0.8% to 5% lanthanum oxide powder, 0.3% to 0.8% yttrium oxide powder, and the remainder is molybdenum powder.
[0035] The average particle size of the molybdenum powder is 3.0-4.0 μm; the particle sizes of the lanthanum oxide powder and the yttrium oxide powder are independently 0.2-2 μm, the purity is independently above 99.95%, and the molybdenum powder, lanthanum oxide powder and yttrium oxide powder do not have single particles with a particle size ≥20 μm.
[0036] In the present invention, the balance means that the remainder is molybdenum powder except for lanthanum oxide powder, yttrium oxide powder, and other components that may be added optionally.
[0037] In the present invention, lanthanum oxide and yttrium oxide can be solid-dissolved with molybdenum at high temperature. Lanthanum oxide and yttrium oxide are dispersed in the molybdenum lattice and grain boundaries, which can modify the grain structure and better pin the movement of dislocations and grain boundaries, thereby improving the recrystallization temperature and tensile properties.
[0038] In the present invention, lanthanum oxide is directly used instead of lanthanum hydroxide because during the sintering process, lanthanum hydroxide will decompose at about 750°C, and the generated water vapor will affect the structure of the grains, and lanthanum hydroxide is prone to produce large particles with a particle size of ≥20μm, resulting in uneven dispersion of lanthanum oxide. Therefore, the present invention directly uses lanthanum oxide, which can avoid the generation of water vapor to affect the grain structure on the one hand, and on the other hand, there are no large particles with a particle size of ≥20μm in the lanthanum oxide, which improves the uniformity of lanthanum oxide dispersion, better refines the grains, increases the density, and improves the tensile properties.
[0039] When the addition amount of lanthanum oxide powder is less than 0.8% or the addition amount of yttrium oxide powder is less than 0.3%, the modification effect on the grain structure of the weight is not obvious; when the addition amount of lanthanum oxide powder is greater than 5% or the addition amount of yttrium oxide powder is greater than 0.8%, the relative density of the weight decreases and the tensile properties decrease. Therefore, in the present invention, the addition amount of the lanthanum oxide powder is, for example, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%; the addition amount of the yttrium oxide powder is, for example, 0.3%, 0.4%, 0.5%, 0.6%, 0.7% or 0.8%.
[0040] In the present invention, when using molybdenum powder with an average particle size of less than 3.0 μm, there are more agglomerates in the molybdenum powder, resulting in low density of the compact and coarse and uneven grains during sintering. When the average particle size is greater than 4.0 μm, the particles are too large and the sintering activity is insufficient, which reduces the density of the sintered compact. Therefore, the average particle size of the molybdenum powder is 3.0 to 4.0 μm. The molybdenum powder of this particle size not only has a moderate agglomeration content, but also has a high sintering activity, which is conducive to the improvement of the weight density; the average particle size of the molybdenum powder is, for example, 3.0 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm, 3.6 μm, 3.7 μm, 3.8 μm, 3.9 μm or 4.0 μm.
[0041] In a preferred embodiment of the present invention, the average particle size of the molybdenum powder is 3.5 μm.
[0042] According to a second aspect of the present invention, a method for preparing a molybdenum-lanthanum oxide-yttrium oxide alloy weight is provided, comprising: mixing various raw materials, and then pressing and sintering to obtain a sintered blank.
[0043] In the present invention, after the sintered blank is obtained, the next step can be carried out without the need for a forging process, so the manufacturing process is simple and the manufacturing cost is saved.
[0044] In a preferred embodiment of the present invention, the raw materials are mixed for 20 to 40 hours. If the mixing time is less than 20 hours, there will be uneven mixing, which will affect the performance; if the mixing time is more than 40 hours, the cost will increase and the efficiency will be delayed.
[0045] In the present invention, the raw material mixing time is, for example, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, 32 h, 34 h, 36 h, 38 h or 40 h.
[0046] In a preferred embodiment of the present invention, the press forming satisfies at least one of the following process parameters:
[0047] (a) Pressing molding adopts cold isostatic pressing;
[0048] (b) cold isostatic pressing at a pressure of 190 to 230 MPa; and
[0049] (c) The holding time is 10 to 30 minutes;
[0050] Specifically, the mixed powder is transferred to a heavy hammer mold, and cold isostatic pressing is performed at 190-230 MPa for 10-30 minutes to obtain a compact. The heavy hammer mold is a rubber sleeve with an inclination at one end, and the initially formed compact is an inclination compact, which can save a certain amount of raw materials.
[0051] In the present invention, the pressure in the press forming step is, for example, 190 MPa, 200 MPa, 210 MPa, 220 MPa or 230 MPa, and the holding time is, for example, 10 min, 13 min, 15 min, 18 min, 20 min, 22 min, 25 min, 27 min or 30 min.
[0052] Preferably, in order to prevent the compact obtained by press forming from swelling and cracking due to moisture absorption, the compact obtained by press forming is vacuum sealed and stored for later use before the next step.
[0053] Furthermore, the sealed compact is stored in an environment with a humidity of ≤20%, and the next step is completed within 24 hours.
[0054] In a preferred embodiment of the present invention, the preparation method further comprises the steps of shaping the pressed product and then sintering it.
[0055] Preferably, the shaping step comprises: shaping the pressed green sheet to obtain a shaped green sheet in an environment with a humidity of ≤20%.
[0056] Specifically, in the present invention, a horizontal lathe is used to shape the green compact.
[0057] Preferably, in order to prevent the shaped blank from swelling and cracking due to moisture absorption, the shaped blank is vacuum-sealed and stored for future use.
[0058] Furthermore, the sealed shaped blank is stored in an environment with a humidity of ≤20%.
[0059] In a preferred embodiment of the present invention, the sintering step includes a first sintering stage, a second sintering stage and a third sintering stage.
[0060] The first sintering stage is to increase the temperature to a first insulation temperature and then keep it for 1 to 4 hours. The first insulation temperature is 180 to 250°C.
[0061] The second sintering stage is to increase the temperature from the first insulation temperature to the second insulation temperature, and then keep it for 1 to 4 hours. The second insulation temperature is 1300 to 1500°C.
[0062] The third sintering stage is to increase the temperature from the second insulation temperature to the sintering temperature and then keep it for 4 to 8 hours. The sintering temperature is 1950 to 2200°C.
[0063] Preferably, the heating rates of the first sintering stage, the second sintering stage and the third sintering stage are independently 50-100° C. / h.
[0064] Specifically, in the present invention, a medium frequency furnace is used for sintering, and a slower heating rate and a higher sintering temperature are used during sintering, which helps to improve the purity of the blank on the one hand, and helps to form a uniform and stable grain structure on the other hand, thereby improving the tensile properties. The heating rate is, for example, 50°C / h, 55°C / h, 60°C / h, 70°C / h, 80°C / h, 90°C / h or 100°C / h.
[0065] In the present invention, the first sintering stage is to remove water adsorbed on the surface of the powder. When the first insulation temperature is lower than 180°C, the water removal rate is too slow, the removal is incomplete, and the grain structure is affected. When the first insulation temperature is greater than 250°C, the water removal rate is too fast, which is easy to form a large pressure, destroy the internal structure of the blank, and finally reduce the tensile properties. The first insulation temperature is, for example, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C or 250°C, and the insulation time of the first sintering stage is, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h.
[0066] The second insulation temperature is used to remove impurities such as O, K, C, Cl, Al, Na, Mg, Ca and Fe. The second insulation temperature is, for example, 1300°C, 1320°C, 1350°C, 1370°C, 1400°C, 1420°C, 1450°C, 1470°C or 1500°C. The insulation time of the second sintering stage is, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h.
[0067] In the third sintering stage of the present invention, molybdenum powder, lanthanum oxide powder and yttrium oxide powder gradually bond with each other, the grains grow, the voids and grain boundaries decrease, the total volume shrinks, and the density increases. When the sintering temperature is lower than 1950°C, the density of the sintered blank does not meet the requirements. When the sintering temperature is higher than 2200°C, overburning is likely to occur, which reduces the tensile properties. The sintering temperature is, for example, 1950°C, 1980°C, 2000°C, 2050°C, 2100°C, 2150°C, 2180°C or 2200°C. When the holding time is less than 4h, the sintering reaction is incomplete. When the holding time is greater than 8h, the grain structure may be damaged due to the long holding time. Therefore, the holding time of the third stage is 4 to 8h, for example, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h.
[0068] Preferably, the sintering step is performed under vacuum or a reducing atmosphere, preferably a hydrogen atmosphere.
[0069] When the hydrogen flow rate is less than 2m 3 / h, the impurities in the raw materials cannot be completely taken away, affecting the final performance; hydrogen is fed from the bottom, when the hydrogen flow rate is greater than 15m 3 / h, the density at the lower end will be lower than that at the upper end, affecting performance and increasing hydrogen costs. Therefore, the hydrogen flow rate is preferably 2 to 15 m 3 / h.
[0070] In a preferred embodiment of the present invention, the preparation method further comprises a step of machining after sintering.
[0071] In the present invention, the molybdenum powder, lanthanum oxide powder and yttrium oxide powder only need to be mixed, pressed, shaped and sintered, and then the sintered blank can be directly machined.
[0072] Preferably, the remaining amount of the sintered green body compared to the finished product made by heavy hammer is 1.5-2 mm on one side.
[0073] In the present invention, after the mixed powder is pressed and shaped by cold isostatic pressing, the obtained shaped blank is close to the size of the finished hammer, and the remaining amount after sintering is 1.5-2mm on one side compared with the finished product, which saves raw materials to the greatest extent. The material cost of the molybdenum-lanthanum oxide-yttrium oxide alloy hammer described in the present invention is reduced by more than 50% compared with the forged pure molybdenum hammer, and it is easier to turn, the machining efficiency can be improved by 50%-100%, and the processing cost can be reduced by 60%-120%. The steps of the preparation method described in the present invention are well coordinated, the overall synergistic effect is obvious, and the operation steps are simple and easy, which is conducive to mass production. The preparation method described in the present invention is also very suitable for large-sized molybdenum alloy hammers, and its appearance specifications can reach φ110*500mm.
[0074] According to a third aspect of the present invention, there is provided an application of a molybdenum-lanthanum oxide-yttrium oxide alloy weight in a single crystal silicon growth furnace.
[0075] The molybdenum-lanthanum oxide-yttrium oxide alloy weight has a service life of more than 1 year in a high temperature environment exceeding 1300°C.
[0076] Example 1
[0077] Preparation of Mo-1%La 2 O 3 -0.4%Y 2 O 3 Alloy weight, the dimensions are Φ90×400mm, the specific steps are as follows:
[0078] (1) 98.6 parts by weight of molybdenum powder with a particle size of 3.7 μm, 1 part by weight of lanthanum oxide with a particle size of 1 μm, and 0.4 parts by weight of yttrium oxide powder with a particle size of 1.5 μm were mixed in a mixer for 24 hours to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy powder.
[0079] (2) The mixed alloy powder is loaded into a heavy hammer mold, and a cold isostatic press is used for cold isostatic pressing. The cold isostatic pressing pressure is 200 MPa, and the holding time is 10 minutes to obtain a preliminarily formed green compact, which is vacuum sealed and stored. The heavy hammer mold is a rubber sleeve with an inclination.
[0080] (3) shaping the pressed green sheet according to the shaping drawing in an environment with a humidity of 18% using a horizontal lathe to obtain a shaped green sheet, and storing the shaped green sheet in a vacuum-sealed manner.
[0081] (4) Sintering the shaped blank in a medium frequency induction heating furnace; sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 5m 3 / h, the heating rate of the entire temperature section is 80℃ / h; first, the temperature is raised to 200℃ and kept at this temperature for 2h; then the temperature is raised to 1300℃ and kept at this temperature for 2h; finally, the temperature is raised to the sintering temperature of 2000℃ and the holding time is 5h to obtain a sintered blank.
[0082] (5) Using a CNC lathe, the sintered blank is directly machined according to the drawing to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy weight.
[0083] Prepare 10 Mo-1% La 2 O 3 -0.4%Y 2 O 3 Alloy weight, measured by hydrostatic weighing method, the actual density average is 9.96g / cm 3 The average relative density is 98.1%. The obtained weight material has uniform and fine grains, with an average grain size of 26μm; the tensile strength is 380MPa, the elongation is 10%, and the average service life is more than 1 year, meeting the life requirements.
[0084] Example 2
[0085] Preparation of Mo-2%La 2 O 3 -0.5% Y 2 O 3 Alloy weight, the dimensions are Φ90×400mm, the specific steps are as follows:
[0086] (1) 97.5 parts by weight of molybdenum powder with a particle size of 3.5 μm, 2 parts by weight of lanthanum oxide with a particle size of 1 μm, and 0.5 parts by weight of yttrium oxide powder with a particle size of 1.5 μm were mixed in a mixer for 30 hours to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy powder.
[0087] (2) The mixed alloy powder is loaded into a heavy hammer mold, and a cold isostatic pressing machine is used for cold isostatic pressing. The cold isostatic pressing pressure is 210 MPa, and the holding time is 20 minutes to obtain a preliminarily formed green compact, which is vacuum sealed and stored. The heavy hammer mold is a rubber sleeve with an inclination.
[0088] (3) Perform shaping according to the shaping drawing using a horizontal lathe in an environment with a humidity of 18% to obtain a shaped blank, and store the shaped blank in a vacuum-sealed manner.
[0089] (4) The shaped blank is sintered in a medium frequency induction heating furnace. The sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 10m 3 / h, the heating rate of the entire temperature section is 70℃ / h; first, the temperature is raised to 200℃ and kept for 2h, then the temperature is raised to 1400℃ and kept for 2h; finally, the temperature is raised to the sintering temperature of 2100℃ and the holding time is 6h to obtain a sintered blank.
[0090] (5) Using a CNC lathe, the sintered blank is directly machined according to the drawing to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy weight.
[0091] Preparation of 10 Mo-2% La strands by the method of Example 2 2 O 3 -0.5% Y 2 O 3 Alloy weight, measured by hydrostatic weighing method, the actual density average is 9.88g / cm 3 The average relative density is 98%. The obtained weight material has uniform and fine grains, with an average grain size of 23μm; the tensile strength is 450MPa, the elongation is 10%, and the average service life is more than 1 year, meeting the life requirements.
[0092] Example 3
[0093] Preparation of Mo-4%La 2 O 3 -0.6%Y 2 O 3 Alloy weight, the dimensions are Φ90×400mm, the specific steps are as follows:
[0094] (1) 95.4 parts by weight of molybdenum powder with a particle size of 3.3 μm, 4 parts by weight of lanthanum oxide with a particle size of 1 μm, and 0.6 parts by weight of yttrium oxide powder with a particle size of 1.5 μm were mixed in a mixer for 36 hours to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy powder.
[0095] (2) The mixed alloy powder is loaded into a heavy hammer mold, and a cold isostatic press is used for cold isostatic pressing. The cold isostatic pressing pressure is 220 MPa, and the holding time is 25 min to obtain a preliminarily formed green compact, which is vacuum sealed and stored. The heavy hammer mold is a rubber sleeve with an inclination.
[0096] (3) Perform shaping according to the shaping drawing using a horizontal lathe in an environment with a humidity of 18% to obtain a shaped blank, and store the shaped blank in a vacuum-sealed manner.
[0097] (4) The shaped blank is sintered in a medium frequency induction heating furnace. The sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 13m 3 / h, the heating rate of the whole temperature section is 60℃ / h; first, the temperature is raised to 200℃ and kept at this temperature for 2h; then, the temperature is raised to 1450℃ and kept at this temperature for 2h; finally, the temperature is raised to the sintering temperature of 2150℃ and the holding time is 7h to obtain a sintered blank.
[0098] (5) Using a CNC lathe, the sintered blank is directly machined according to the drawing to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy weight.
[0099] Prepare 10 Mo-4% La wires by the method of Example 3 2 O 3 -0.6%Y 2 O 3 Alloy weight, measured by hydrostatic weighing method, the actual density average is 9.8g / cm 3 The average relative density is 98.5%. The obtained weight material has uniform and fine grains, with an average grain size of 15μm; the tensile strength is 500MPa, the elongation is 10%, and the average service life is more than 1 year, meeting the life requirements.
[0100] Example 4
[0101] Preparation of Mo-2%La 2 O 3 -0.5% Y 2 O 3 Alloy weight, the dimensions are Φ90×400mm, the specific steps are as follows:
[0102] (1) 97.5 parts by weight of molybdenum powder with a particle size of 3.5 μm, 2 parts by weight of lanthanum oxide with a particle size of 1 μm, and 0.5 parts by weight of yttrium oxide powder with a particle size of 1.5 μm were mixed in a mixer for 30 hours to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy powder.
[0103] (2) The mixed alloy powder is loaded into a heavy hammer mold, and a cold isostatic pressing machine is used for cold isostatic pressing. The cold isostatic pressing pressure is 210 MPa, and the holding time is 20 minutes to obtain a preliminarily formed green compact, which is vacuum sealed and stored. The heavy hammer mold is a rubber sleeve with an inclination.
[0104] (3) According to the shaping drawing, shaping is performed using a horizontal lathe in an environment with a humidity of 18% to obtain a shaped blank, and the shaped blank is vacuum-sealed and stored.
[0105] (4) The shaped blank is sintered in a medium frequency induction heating furnace. The sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 10m 3 / h, the heating rate of the entire temperature section is 150℃ / h; first, the temperature is raised to 400℃ and kept for 2h, then the temperature is raised to 1200℃ and kept for 2h; finally, the temperature is raised to the sintering temperature of 1900℃ and the holding time is 6h to obtain a sintered blank.
[0106] (5) Using a CNC lathe, the sintered blank is directly machined according to the drawing to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy weight.
[0107] 10 Mo-2% La were prepared using the method of Example 4 2 O 3 -0.5% Y 2 O 3 Alloy weight, measured by hydrostatic weighing method, the actual density average is 9.84g / cm 3 The average relative density is 97.6%. The obtained weight material has small grains but holes, and the average grain size is 18μm; the tensile strength is 320MPa, the elongation is 5%, and the average service life is 1 year, which meets the life requirements.
[0108] Comparative Example 1
[0109] Preparation of Mo-2%La 2 O 3 -0.5% Y 2 O 3 Alloy weight, the dimensions are Φ90×400mm, the specific steps are as follows:
[0110] (1) 97.5 parts by weight of molybdenum powder with a particle size of 3.5 μm, 2 parts by weight of lanthanum hydroxide with a particle size of 1 μm, and 0.5 parts by weight of yttrium oxide powder with a particle size of 1.5 μm were mixed in a mixer for 30 hours to obtain a molybdenum-lanthanum hydroxide-yttrium oxide alloy powder.
[0111] (2) The mixed alloy powder is loaded into a heavy hammer mold, and a cold isostatic pressing machine is used for cold isostatic pressing. The cold isostatic pressing pressure is 210 MPa, and the holding time is 20 minutes to obtain a preliminarily formed green compact, which is vacuum sealed and stored. The heavy hammer mold is a rubber sleeve with an inclination.
[0112] (3) shaping the pressed green sheet according to the shaping drawing in an environment with a humidity of 18% using a horizontal lathe to obtain a shaped green sheet, and storing the shaped green sheet in a vacuum-sealed manner.
[0113] (4) The shaped blank is sintered in a medium frequency induction heating furnace. The sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 10m 3 / h, the heating rate of the whole temperature section is 70℃ / h, and the insulation time at 200℃ and 1400℃ is 2h respectively; the sintering temperature is 2100℃, and the insulation time is 6h to obtain a sintered blank.
[0114] (5) Using a CNC lathe, the sintered blank is directly machined according to the drawing to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy weight.
[0115] Comparative Example 1 Preparation of 10 Mo-2% La 2 O 3 -0.5% Y 2 O 3The average actual density of the alloy weight measured by hydrostatic weighing method is 9.87g / cm 3 The average relative density is 97.9%. The average grain size of the obtained weight material is 24μm, and there is an 80μm large particle O-La-Y dispersed phase in the dispersed phase; its tensile strength is 290MPa, elongation is 8%, and the average service life is 8 months, which does not meet the life requirement.
[0116] Comparative Example 2
[0117] Prepare a pure molybdenum weight with dimensions of Φ90×400mm. The specific steps are as follows:
[0118] (1) 100 parts by weight of molybdenum powder with a particle size of 3.5 μm was batch-processed in a mixer for 30 hours.
[0119] (2) Molybdenum powder is loaded into a heavy hammer mold and cold isostatic pressing is performed using a cold isostatic press. The cold isostatic pressing pressure is 210 MPa and the holding time is 20 min to obtain a preliminarily formed green compact. The green compact is vacuum sealed and stored. The heavy hammer mold is a rubber sleeve with an inclination.
[0120] (3) Perform shaping according to the shaping drawing using a horizontal lathe in an environment with a humidity of 18% to obtain a shaped blank, and store the shaped blank in a vacuum-sealed manner.
[0121] (4) Sintering the shaped blank in a medium frequency induction heating furnace; sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 10m 3 / h, the heating rate of the entire temperature section is 70℃ / h; first, the temperature is raised to 200℃ and kept for 2h, then the temperature is raised to 1400℃ and kept for 2h; finally, the temperature is raised to the sintering temperature of 2100℃ and the holding time is 6h to obtain a sintered blank.
[0122] (5) Use a CNC lathe to directly machine the sintered blank according to the drawing to obtain a pure molybdenum weight.
[0123] Ten pure molybdenum weights were prepared by the method of Comparative Example 2. The average actual density was measured by hydrostatic weighing method and was 10 g / cm 3 The average relative density is 97.6%. The obtained weight material has uniform grains, an average grain size of 36μm, a tensile strength of 200MPa, an elongation of 8%, and an average service life of 2 months, which does not meet the life requirements.
[0124] Comparative Example 3
[0125] Prepare a pure molybdenum weight with dimensions of Φ90×400mm. The specific steps are as follows:
[0126] (1) 100 parts by weight of molybdenum powder having a particle size of 3.8 μm was batched in a mixer.
[0127] (2) Molybdenum powder is placed in a heavy hammer mold for cold isostatic pressing at a pressure of 210 MPa and a holding time of 20 min to obtain a preliminarily formed green compact, which is then sealed in a vacuum and stored.
[0128] (3) Perform shaping according to the shaping drawing using a horizontal lathe in an environment with a humidity of 18% to obtain a shaped blank, and store the shaped blank in a vacuum-sealed manner.
[0129] (4) Sintering the shaped blank in a medium frequency induction heating furnace; sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 10m 3 / h, the heating rate of the whole temperature section is 70℃ / h; first, the temperature is raised to 200℃ and kept for 2h, then the temperature is raised to 1400℃ and kept for 2h; finally, the temperature is raised to the sintering temperature of 2100℃ and kept for 6h to obtain a sintered blank. The diameter of the sintered blank is 130mm.
[0130] (5) After forging the sintered blank at 1350° C. using an air hammer, the blank was processed using a CNC lathe according to the drawing to obtain a pure molybdenum weight with a size of Φ90×400 mm.
[0131] Ten pure molybdenum weights were prepared using the method of Comparative Example 3, and the average actual density was measured by hydrostatic weighing method, which was 10.18 g / cm 3 The average relative density is 99.3%. The longitudinal section of the obtained weight material is a fibrous structure grain, and the cross-sectional grain size is 3 μm; the tensile strength is 600 MPa, the elongation is 20%, and the average service life is greater than 1 year, which meets the life requirement, but the cost is 1.6 times that of Example 2.
[0132] Comparative Example 4
[0133] Preparation of Mo-2%La 2 O 3 -0.5% Y 2 O 3 Alloy weight, the dimensions are Φ90×400mm, the specific steps are as follows:
[0134] (1) 97.5 parts by weight of molybdenum powder with a particle size of 2 μm, 2 parts by weight of lanthanum oxide with a particle size of 1 μm, and 0.5 parts by weight of yttrium oxide powder with a particle size of 1.5 μm were mixed in a mixer for 30 hours to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy powder.
[0135] (2) The mixed alloy powder is loaded into a heavy hammer mold, and a cold isostatic pressing machine is used for cold isostatic pressing. The cold isostatic pressing pressure is 210 MPa, and the holding time is 20 minutes to obtain a preliminarily formed green compact, which is vacuum sealed and stored. The heavy hammer mold is a rubber sleeve with an inclination.
[0136] (3) Perform shaping according to the shaping drawing using a horizontal lathe in an environment with a humidity of 18% to obtain a shaped blank, and store the shaped blank in a vacuum-sealed manner.
[0137] (4) The shaped blank is sintered in a medium frequency induction heating furnace. The sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 10m 3 / h, the heating rate of the entire temperature section is 70℃ / h; first, the temperature is raised to 200℃ and kept for 2h, then the temperature is raised to 1400℃ and kept for 2h; finally, the temperature is raised to the sintering temperature of 2100℃ and the holding time is 6h to obtain a sintered blank.
[0138] (5) Using a CNC lathe, the sintered blank is directly machined according to the drawing to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy weight.
[0139] Comparative Example 4 method to prepare 10 Mo-2% La 2 O 3 -0.5% Y 2 O 3 Alloy weight, measured by hydrostatic weighing method, the actual density average is 9.80g / cm 3 The average relative density is 97.2%. The obtained weight material has large and uneven grains, with an average grain size of 32μm; the tensile strength is 290MPa, the elongation is 7%, and the average service life is 10 months, which does not meet the life requirement.
[0140] Comparative Example 5
[0141] Preparation of Mo-2%La 2 O 3 -0.5% Y 2 O 3 Alloy weight, the dimensions are Φ90×400mm, the specific steps are as follows:
[0142] (1) 97.5 parts by weight of molybdenum powder with a particle size of 5 μm, 2 parts by weight of lanthanum oxide with a particle size of 1 μm, and 0.5 parts by weight of yttrium oxide powder with a particle size of 1.5 μm were mixed in a mixer for 30 hours to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy powder.
[0143] (2) The mixed alloy powder is loaded into a heavy hammer mold, and a cold isostatic pressing machine is used for cold isostatic pressing. The cold isostatic pressing pressure is 210 MPa, and the holding time is 20 minutes to obtain a preliminarily formed green compact, which is vacuum sealed and stored. The heavy hammer mold is a rubber sleeve with an inclination.
[0144] (3) Perform shaping according to the shaping drawing using a horizontal lathe in an environment with a humidity of 18% to obtain a shaped blank, and store the shaped blank in a vacuum-sealed manner.
[0145] (4) The shaped blank is sintered in a medium frequency induction heating furnace. The sintering is carried out in a hydrogen atmosphere with a hydrogen flow rate of 10m 3 / h, the heating rate of the entire temperature section is 70℃ / h; first, the temperature is raised to 200℃ and kept for 2h, then the temperature is raised to 1400℃ and kept for 2h; finally, the temperature is raised to the sintering temperature of 2100℃ and the holding time is 6h to obtain a sintered blank.
[0146] (5) Using a CNC lathe, the sintered blank is directly machined according to the drawing to obtain a molybdenum-lanthanum oxide-yttrium oxide alloy weight.
[0147] Comparative Example 5 method to prepare 10 Mo-2% La 2 O 3 -0.5% Y 2 O 3 The average actual density of the alloy weight measured by hydrostatic weighing method is 9.73 g / cm 3 The average relative density is 96.5%. The obtained weight material has coarse grains, with an average grain size of 26μm; the tensile strength is 280MPa, the elongation is 9%, and the average service life is 10 months, which does not meet the life requirement.
[0148] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.
Claims
1. A molybdenum-lanthanum oxide-yttrium oxide alloy weight, characterized in that: The weight is made of the following raw materials in percentage by weight: 0.8% to 5% lanthanum oxide powder, 0.3% to 0.8% yttrium oxide powder, and the balance is molybdenum powder; The average particle size of the molybdenum powder is 3.0-4.0 μm; the particle sizes of the lanthanum oxide powder and the yttrium oxide powder are independently 0.2-2 μm, and the molybdenum powder, lanthanum oxide powder and yttrium oxide powder do not contain single particles with a particle size of ≥20 μm; The preparation method of the molybdenum-lanthanum oxide-yttrium oxide alloy weight comprises: mixing various raw materials, and then sequentially performing pressing, shaping, sintering and machining; The green compact obtained by pressing is vacuum sealed and stored for later use; In an environment with a humidity of ≤20%, shaping the compact to obtain a shaped compact, and vacuum-sealing the shaped compact for storage; The sintering step includes a first sintering stage, a second sintering stage and a third sintering stage; The first sintering stage is to increase the temperature to the first insulation temperature and keep it for 1 to 4 hours, and the first insulation temperature is 180 to 250° C.; The second sintering stage is to increase the temperature from the first insulation temperature to the second insulation temperature, and then keep the temperature for 1 to 4 hours, and the second insulation temperature is 1300 to 1500° C.; The third sintering stage is to increase the temperature from the second insulation temperature to the sintering temperature and keep it for 4 to 8 hours, and the sintering temperature is 1950 to 2200°C; The heating rates of the first sintering stage, the second sintering stage and the third sintering stage are independently 50-100° C. / h.
2. The weight according to claim 1, characterized in that: The average particle size of the molybdenum powder is 3.5 μm.
3. The weight according to claim 1, characterized in that: The time for mixing the raw materials is 20 to 40 hours.
4. The weight according to claim 1, characterized in that: The pressing process is performed by cold isostatic pressing and at least one of the following process parameters is met: (b) cold isostatic pressing at a pressure of 190 to 230 MPa; and (c) The holding time is 10 to 30 minutes.
5. The weight according to claim 1, characterized in that: The sintering step is performed under vacuum or a reducing atmosphere.
6. The weight according to claim 5, characterized in that: The sintering step is performed under a hydrogen atmosphere.
7. The weight according to claim 6, characterized in that: The hydrogen flow rate is 2 to 15 m 3 / h.
8. The weight according to claim 1, characterized in that: The allowance of the sintered blank compared to the finished product made by heavy hammer is 1.5 to 2 mm on one side.
9. Use of the molybdenum-lanthanum oxide-yttrium oxide alloy weight as claimed in any one of claims 1 to 8 in a single crystal silicon growth furnace.
Citation Information
Patent Citations
High-strength Mo-doped sheet and preparation method thereof
CN101935793A
Preparation method for molybdenum blank for preparing metal molybdenum wire
CN108546840A
High-strength molybdenum alloy rod and preparation method thereof
CN111041314A
Preparation method of dry-type molybdenum-doped alloy
CN113600815A
Nano yttrium oxide dispersion strengthened molybdenum alloy and preparation method thereof
CN113737040A