Method for producing lithium nickel composite oxide
By adjusting the molar ratio of the filler during the manufacturing process of the lithium-nickel composite oxide, the consistency of the crystallite size of the lithium-nickel composite oxide is ensured, the problem of crystallite size deviation of the lithium-nickel composite oxide is solved, and the non-aqueous Discharge performance of electrolyte secondary batteries.
Patent Information
- Application Number
- CN202180063929.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-25
- Filing Date
- 2021-09-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-09-13
AI Technical Summary
In the existing manufacturing method of lithium-nickel composite oxide, heat conduction during firing is insufficient, resulting in deviations in the crystallite size of the lithium-nickel composite oxide, which affects the discharge rate characteristics of non-aqueous electrolyte secondary batteries.
When the Ni-containing metal compound and the Li compound are filled in the firing container and divided into two halves in the height direction, the molar ratio A of Li to metals other than Li in the upper half region and the molar ratio A of Li in the lower half region are ensured. The molar ratio B of Li to metals other than Li satisfies 1
Through this method, a lithium-nickel composite oxide with small variation in crystallite size is obtained, and the discharge rate characteristics of the non-aqueous electrolyte secondary battery are improved.
Smart Images

Figure CN116195096B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a lithium nickel composite oxide. Background Art
[0002] Non-aqueous electrolyte secondary batteries represented by lithium ion secondary batteries have been used as power sources for portable electronic devices because of their high energy density. In addition, not limited to the above-mentioned uses, non-aqueous electrolyte secondary batteries are also being researched and developed with the goal of being used as large power sources for hybrid vehicles, electric vehicles, etc.
[0003] Lithium nickel composite oxide used as positive electrode active material of non-aqueous electrolyte secondary batteries has advantages such as higher capacity than the currently mainstream lithium cobalt composite oxide, nickel as a raw material is cheaper than cobalt, and can be obtained stably. Therefore, it is expected to be the next generation positive electrode material.
[0004] Examples of methods for producing lithium nickel composite oxides include a method in which a cathode material precursor powder containing lithium and nickel is filled in a calcination container and calcined for a predetermined time in an oxygen atmosphere or an air atmosphere (eg, Patent Document 1).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 5916876 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, in the existing method for manufacturing lithium nickel composite oxides, heat conduction during calcination is insufficient, so the reaction is not fully carried out near the bottom surface of the calcination container, and there is a problem that the crystallite size of the obtained lithium nickel composite oxide has a large deviation. If a lithium nickel composite oxide with a large deviation in crystallite size is used as a positive electrode active material, there is a concern that the discharge rate characteristics of a non-aqueous electrolyte secondary battery will be reduced, so a manufacturing method for suppressing the deviation in crystallite size of the lithium nickel composite oxide is sought.
[0010] Therefore, an object of the present invention is to provide a method for producing a lithium nickel composite oxide capable of suppressing the variation in crystallite size.
[0011] Means used to solve problems
[0012] A method for producing a lithium nickel composite oxide in one embodiment of the present invention includes: a filling step of filling a Ni-containing metal compound and a Li compound in a calcining container to obtain a filling containing the above-mentioned Ni-containing metal compound and the above-mentioned Li compound; and a calcining step of calcining the above-mentioned filling filled in the above-mentioned calcining container, when the above-mentioned filling filled in the above-mentioned calcining container in the above-mentioned filling step is divided into two equal parts in the height direction, the molar ratio A of Li in the filling in the upper half area to the metal other than Li, and the molar ratio B of Li in the filling in the lower half area to the metal other than Li satisfy 1<B / A<1.15.
[0013] Effects of the Invention
[0014] According to one embodiment of the present invention, a lithium nickel composite oxide with suppressed variation in crystallite size can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic cross-sectional view of a calcining container filled with a Ni-containing metal compound and a Li compound.
[0016] Figure 2 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of an embodiment. DETAILED DESCRIPTION
[0017] Hereinafter, an example of the embodiment will be described in detail with reference to the drawings. The drawings referred to in the description of the embodiment are drawings for schematic description.
[0018] The method for producing the lithium nickel composite oxide of the present embodiment includes: a filling step of filling a calcining container with a Ni-containing metal compound and a Li compound to obtain a filling material containing the Ni-containing metal compound and the Li compound; and a calcining step of calcining the filling material containing the Ni-containing metal compound and the Li compound filled in the calcining container.
[0019] <Filling process>
[0020] The Ni-containing metal compound filled in the calcination container is not particularly limited as long as it is a Ni-containing compound, and may also contain other elements other than Ni. As other elements, for example, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, etc. Among them, it is preferred to contain at least one of Co, Mn, and Al. As an example of a preferred compound, a metal compound containing Ni, Co, and Mn, a metal compound containing Ni, Co, and Al, etc. can be cited. The Ni-containing metal compound is, for example, in the form of hydroxides, oxyhydroxides, oxides, etc. Among these, from the perspective of the ease of compounding Ni with elements other than it, or the high reactivity with Li compounds, it is preferably in the form of hydroxides and oxyhydroxides. Ni-containing metal hydroxides are obtained, for example, by crystallization, coprecipitation, uniform precipitation, and other previously known methods. In addition, Ni-containing metal oxyhydroxides are obtained, for example, by adding oxidants such as sodium hypochlorite and hydrogen peroxide to the Ni-containing metal hydroxide obtained by the above-mentioned method. The Ni-containing metal oxide is obtained, for example, by calcining the above-mentioned hydroxide or oxyhydroxide in a non-reducing atmosphere. The calcination temperature is not particularly limited as long as the non-reducing atmosphere can be maintained, but is preferably 850°C or less, and more preferably in the range of 500°C to 750°C.
[0021] The Li compound filled in the calcining container can include, for example, hydroxides, oxyhydroxides, oxides, carbonates, nitrates and halides of lithium. These Li compounds can be used alone or in combination. Among these, lithium hydroxides are preferred, particularly lithium hydroxides, from the perspective of low melting point and high reactivity with Ni-containing metal compounds.
[0022] Figure 1Schematic cross-sectional view of a calcining container filled with a Ni-containing metal compound and a Li compound. When the filler 5 containing a Ni-containing metal compound and a Li compound filled in the calcining container 7 in the filling step is divided into two equal parts in the height direction, the molar ratio A of Li to metals other than Li in the filler 5a in the upper half region and the molar ratio B of Li to metals other than Li in the filler 5b in the lower half region satisfy 1<B / A<1.15. That is, the Ni-containing metal compound and the Li compound must be filled in the calcining container 7 in such a way that the molar ratio A and the molar ratio B satisfy 1<B / A<1.15. As a filling method that satisfies the above range, for example, a method can be cited in which the Li compound is filled from the bottom surface of the calcining container 7 to a predetermined height, and a mixture of the Ni-containing metal compound and the Li compound is filled to a predetermined height on the filled Li compound. The Li compound initially filled in the calcining container 7 and the Li compound of the mixture filled thereafter may be the same compound or different compounds. When different compounds are used, the Li compound initially filled in the calcining container 7 is preferably a Li compound having a low melting point, particularly a Li compound having a lower melting point than the Li compound of the mixture to be filled later.
[0023] In addition, for example, a mixture of Ni-containing metal compounds and Li compounds can be filled in such a way that the molar ratio of Li to metals other than Li is gradually increased from the top surface of the filler 5 filled in the calcining container 7 toward the bottom surface. Specifically, a mixture A of Ni-containing metal compounds and Li compounds having a high molar ratio of Li to metals other than Li is filled from the bottom surface of the calcining container 7 to a predetermined height, and on the mixture A, a mixture B of Ni-containing metal compounds and Li compounds having a lower molar ratio of Li to metals other than Li than the mixture A is filled to a predetermined height. In addition, on the mixture B, a mixture C of Ni-containing metal compounds and Li compounds having a lower molar ratio of Li to metals other than Li than the mixture B is filled to a predetermined height. Moreover, the filling of the mixture having a lower molar ratio of Li to metals other than Li than the mixture filled so far is continued until the filling reaches a predetermined height. It should be noted that the Li compounds of each mixture may be the same compound or different compounds. When different compounds are used, the Li compound of the mixture initially filled in the calcining container 7 is preferably a Li compound with a low melting point, particularly a Li compound with a lower melting point than the Li compound of the mixture filled later. The above-mentioned filling method is an example, and the Ni-containing metal compound and the Li compound can be filled in the calcining container 7 in any manner as long as the molar ratio A and the molar ratio B satisfy 1<B / A<1.15.
[0024] The molar ratio A and the molar ratio B satisfy 1<B / A<1.15, which means that the amount of Li compound in the filler 5b present in the lower half area is greater than the amount of Li compound in the filler 5a present in the upper half area. In this way, by increasing the amount of Li compound in the filler 5b present in the lower half area, the reactivity near the bottom surface of the calcining container 7 is improved in the calcining process described later, so that a lithium nickel composite oxide with suppressed crystallite size deviation can be obtained. Furthermore, the discharge rate characteristics of the non-aqueous electrolyte secondary battery can be improved. It should be noted that when B / A is 1.15 or more, the amount of Li compound in the filler 5b present in the lower half area becomes excessive, and the unreacted Li compound increases, so the deviation of the crystallite size of the obtained lithium nickel composite oxide cannot be fully suppressed.
[0025] From the viewpoint of further suppressing the variation in the crystallite size, the molar ratio A and the molar ratio B preferably satisfy, for example, 1.02≤B / A≤1.12.
[0026] The molar ratio of Li in the whole filler to the metal other than Li, the molar ratio of Ni to the metal other than Li, etc. are appropriately set according to the composition of the lithium nickel composite oxide as the target. However, for example, from the perspective of thermal stability, the molar ratio of Li in the whole filler to the metal other than Li is preferably 0.95 or more and 1.10 or less. In addition, for example, from the perspective of capacity, the molar ratio of Ni in the whole filler to the metal other than Li is preferably 0.65 or more and 1.00 or less.
[0027] As the calcination container 7 in the industrial production process, for example, a container with inner dimensions in the range of 100 mm (L) × 100 mm (W) × 20 mm (H) to 500 mm (L) × 500 mm (W) × 100 mm (H) is used. And the raw material is filled in such a way that the height of the filler 5 containing the Li compound and the Ni-containing metal compound as the raw material is, for example, in the range of 5 to 100 mm.
[0028] <Firing process>
[0029] The filler 5 containing the Ni-containing metal compound and the Li compound filled in the calcination container 7 is calcined. The calcination conditions are appropriately set in consideration of the reactivity of the Li compound and the Ni-containing metal compound, and include, for example, a one-stage calcination in which calcination is performed at a temperature in the range of 650 to 850° C. for a predetermined time in an oxygen atmosphere; a two-stage calcination in which calcination is performed at a temperature in the range of 400 to 600° C. for a predetermined time in an oxygen atmosphere, and then calcined at a temperature in the range of 650 to 850° C. for a predetermined time.
[0030] The device for firing the filling material 5 filled in the firing container 7 is not particularly limited, and for example, a firing furnace such as an electric furnace, a kiln, a tubular furnace, or a pusher furnace can be used.
[0031] The fired filling material (fired material) is washed to remove impurities, or pulverized to control the particle size to a predetermined value, as required.
[0032] The manufacturing method of this embodiment can obtain a lithium nickel composite oxide with suppressed crystallite size deviation. The composition of the lithium nickel composite oxide is changed by adjusting the injection amount of the raw materials. For example, from the perspective of increasing the capacity of the non-aqueous electrolyte secondary battery, it is preferred to prepare a composite oxide represented by the following composition formula (1).
[0033] Composition formula (1): Li a Ni 1-b M b O2 (wherein, M represents a metal element other than Ni, a is 0.95≤a≤1.10, and b is 0.01≤b≤0.5.)
[0034] Figure 2 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of an embodiment. Figure 2 The non-aqueous electrolyte secondary battery 10 shown in the figure comprises: a wound electrode body 14 in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween, a non-aqueous electrolyte, insulating plates 18 and 19 respectively arranged above and below the electrode body 14, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a case body 16 in a cylindrical shape with a bottom, and a sealing body 17 for blocking the opening of the case body 16. It should be noted that other types of electrode bodies such as a laminated electrode body in which a positive electrode and a negative electrode are alternately laminated with a separator interposed therebetween may be used instead of the wound electrode body 14. In addition, as the battery case 15, examples include cylindrical, square, coin-shaped, button-shaped, and other metal outer cans, and bag-type outer bodies formed by laminating resin sheets and metal sheets, etc.
[0035] The case body 16 is, for example, a metal outer can with a bottomed cylindrical shape. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure the airtightness of the battery interior. The case body 16 has, for example, a bulging portion 22 in which a part of the side surface bulges inwardly to support the sealing body 17. The bulging portion 22 is preferably formed annularly along the circumference of the case body 16, and supports the sealing body 17 on its upper surface.
[0036] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective central portions, and the insulating member 25 is sandwiched between the respective peripheral portions. If the internal pressure of the non-aqueous electrolyte secondary battery 10 rises due to heat caused by an internal short circuit, for example, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 to the cover 27 side, and the current path between the lower valve body 24 and the upper valve body 26 is blocked. If the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cover 27.
[0037] exist Figure 2 In the non-aqueous electrolyte secondary battery 10 shown, the positive electrode lead 20 attached to the positive electrode 11 passes through the through hole of the insulating plate 18 and extends to the sealing body 17 side, and the negative electrode lead 21 attached to the negative electrode 12 passes through the outside of the insulating plate 19 and extends to the bottom side of the case body 16. The positive electrode lead 20 is connected to the bottom plate of the sealing body 17, that is, the lower surface of the filter 23, by welding or the like, and the top plate of the sealing body 17, that is, the cover 27 electrically connected to the filter 23, becomes the positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the case body 16 by welding or the like, and the case body 16 becomes the negative terminal.
[0038] Hereinafter, each component of the nonaqueous electrolyte secondary battery 10 will be described in detail.
[0039] [negative electrode]
[0040] The negative electrode 12 includes, for example, a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector.
[0041] The negative electrode current collector is made of, for example, a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film having the metal disposed on the surface.
[0042] The negative electrode active material layer contains a negative electrode active material. In addition, the negative electrode active material layer preferably contains a binder, etc. The negative electrode 12 can be made, for example, by preparing a negative electrode mixture slurry containing a negative electrode active material, a binder, etc., applying the negative electrode mixture slurry on a negative electrode collector and drying it to form a negative electrode active material layer, and rolling the negative electrode active material layer.
[0043] There are no particular restrictions on the negative electrode active material as long as it can absorb and release lithium ions. Examples include carbonaceous materials such as natural graphite and artificial graphite, elements such as silicon, titanium, germanium, tin, lead, zinc, magnesium, sodium, aluminum, potassium, indium, alloys, or oxides.
[0044] Examples of the binder include fluorine resins, PAN, polyimide resins, acrylic resins, polyolefin resins, styrene-butadiene rubber (SBR), nitrile rubber (NBR), carboxymethyl cellulose (CMC) or its salts, polyacrylic acid (PAA) or its salts (partially neutralized salts such as PAA-Na and PAA-K may be used), polyvinyl alcohol (PVA), etc. These binders may be used alone or in combination of two or more.
[0045] [positive electrode]
[0046] The positive electrode 11 is composed of, for example, a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode current collector may be a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, or a film having the metal disposed on the surface. The positive electrode active material layer may include, for example, a positive electrode active material, a binder, a conductive agent, and the like.
[0047] The positive electrode 11 can be produced, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive agent, etc., on a positive electrode current collector and drying the slurry to form a positive electrode active material layer, and then rolling the positive electrode active material layer.
[0048] As the positive electrode active material, the lithium nickel composite oxide obtained by the manufacturing method of the present embodiment is used. It should be noted that, within the range that does not damage the battery performance, composite oxides other than the lithium nickel composite oxide obtained by the manufacturing method of the present embodiment may be included. For example, composite oxides that do not contain Ni may be mentioned.
[0049] Examples of the conductive agent include carbon black (CB), acetylene black (AB), Ketjen black, graphite and other carbon particles, etc. These conductive agents may be used alone or in combination of two or more.
[0050] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide-based resins, acrylic resins, and polyolefin-based resins. These binders may be used alone or in combination of two or more.
[0051] [Non-aqueous electrolyte]
[0052] The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The electrolyte is not limited to a liquid electrolyte, and may be a solid electrolyte using a gel-like polymer or the like. The non-aqueous solvent may include, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen substituted product in which at least a portion of the hydrogen in these solvents is substituted by a halogen atom such as fluorine.
[0053] Examples of the above-mentioned esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate, chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate, cyclic carboxylates such as γ-butyrolactone (GBL) and γ-valerolactone (GVL), and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate.
[0054] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ether, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl ether, and the like. Alkenyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether and other chain ethers, etc.
[0055] As the halogen-substituted product, preferably used are fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, fluorinated chain carboxylates such as fluoromethyl propionate (FMP), and the like.
[0056] The electrolyte salt is preferably a lithium salt. Examples of lithium salts include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1<x<6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lower aliphatic carboxylic acid lithium, Li2B4O7, Li(B(C2O4)F2) and other borates, LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1SO2) {l, m is an integer greater than 0} and other imide salts. The lithium salt may be used alone or in combination. Among these, LiPF6 is preferably used from the viewpoints of ion conductivity and electrochemical stability. The concentration of the lithium salt is preferably set to 0.8 to 1.8 mol per 1 L of the non-aqueous solvent.
[0057] [Spacer]
[0058] For example, the spacer 13 may be a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the spacer, olefin resins such as polyethylene and polypropylene, cellulose, etc. are preferred. The spacer 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, it may be a multilayer spacer including a polyethylene layer and a polypropylene layer, or a spacer having a material such as an aramid resin or ceramics coated on the surface of the spacer may be used.
[0059] Example
[0060] Hereinafter, the present invention will be further described by way of examples, but the present invention is not limited to these examples.
[0061] <Example 1>
[0062] [Preparation of lithium nickel composite oxide]
[0063] Urea is added to a mixed solution containing nickel sulfate, cobalt sulfate and aluminum nitrate, and the solution is stirred while the solution temperature is adjusted to between 80 and 100°C to control the crystal growth rate to obtain a precipitate. The precipitate is a Ni-Co-Al coprecipitated hydroxide (Ni) with an atomic ratio of Ni, Co and Al of 0.91:0.045:0.045. 0.91 Co 0.045 Al 0.045 (OH)2).
[0064] Next, the Ni—Co—Al coprecipitated hydroxide is mixed with lithium hydroxide monohydrate (LiOH / H 2 O) to obtain a mixed powder M.
[0065] The bottom surface of the alumina calcining container is filled with lithium hydroxide monohydrate, and the mixed powder M is filled on the filled lithium hydroxide monohydrate, so that a filling is formed in the calcining container. The ratio of the lithium hydroxide monohydrate filled on the bottom surface of the calcining container and the mixed powder M filled on the lithium hydroxide monohydrate is set to 5:100 in terms of mass conversion. The mixing ratio of the Ni-Co-Al coprecipitated hydroxide and the lithium hydroxide monohydrate in the mixed powder M is adjusted so that the molar ratio A of Li in the filling to the metal other than Li in the upper half area when the filling is divided into two equal parts in the height direction becomes 1.173, and the molar ratio B of Li in the filling to the metal other than Li in the lower half area becomes 1.314. At this time, the molar ratio B / molar ratio A is 1.12.
[0066] The calcination container with the filling was placed in an electric furnace and calcined at 750° C. for 15 hours in an oxygen atmosphere to obtain a lithium nickel composite oxide containing Co and Al (composition: LiNi 0.91 Co 0.045 Al 0.045 O2). It is used as a positive electrode active material.
[0067] [Production of positive electrode]
[0068] The lithium nickel composite oxide as the positive electrode active material, acetylene black as the conductive agent, and polyvinylidene fluoride (average molecular weight 1.1 million) as the binder were mixed at a mass ratio of 98:1:1 to prepare a positive electrode mixture slurry with a solid content of 70%. The slurry was applied to both sides of an aluminum foil with a thickness of 15 μm, and after the coating was dried, the coating was rolled by a calendering roller, thereby preparing a positive electrode having a positive electrode active material layer formed on both sides of the positive electrode collector.
[0069] [Production of negative electrode]
[0070] The graphite powder is mixed in a manner such that it becomes 95 parts by mass and the Si oxide is mixed in a manner such that it becomes 5 parts by mass, and this is used as a negative electrode active material. 100 parts by mass of the negative electrode active material, 1 part by mass of carboxymethyl cellulose (CMC) as a binder, and an appropriate amount of water are added to the mixture, and 1.2 parts by mass of styrene butadiene rubber (SBR) and an appropriate amount of water are added to prepare a negative electrode mixture slurry. The slurry is applied to both sides of a copper foil having a thickness of 8 μm, and after the coating film is dried, the coating film is rolled by a calendering roller to prepare a negative electrode having a negative electrode active material layer formed on both sides of the negative electrode collector.
[0071] [Preparation of non-aqueous electrolyte]
[0072] To 100 parts by mass of a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) (EC:DMC=1:3 by volume ratio) was added 5 parts by mass of vinylene carbonate (VC), and LiPF6 was dissolved at a concentration of 1 mol / L to prepare a non-aqueous electrolyte.
[0073] [Fabrication of non-aqueous electrolyte secondary battery]
[0074] After the positive electrode and the negative electrode are respectively installed with leads, a spacer with a 3 μm aluminum oxide particle layer formed on a 12 μm polyethylene film is wound between the positive electrode and the negative electrode to make a wound electrode body. The electrode body is inserted into the shell body, and the negative electrode lead is welded to the bottom surface of the shell body. Next, the positive electrode lead is welded to the sealing body. Then, after the non-aqueous electrolyte is injected into the shell body, the open end of the shell body is sealed with a sealing body through a sealing gasket to obtain a non-aqueous electrolyte secondary battery. The battery capacity of the non-aqueous electrolyte secondary battery is 2500mAh.
[0075] <Example 2>
[0076] The ratio of lithium hydroxide monohydrate filled on the bottom surface of the sintering container to the mixed powder M filled on the lithium hydroxide monohydrate is set to 0.1:100 in terms of mass conversion, and a filling is formed in the sintering container. The mixing ratio of Ni-Co-Al coprecipitated hydroxide and lithium hydroxide monohydrate in the mixed powder M is adjusted so that the molar ratio A of Li in the filling in the upper half area when the filling is divided into two equal parts in the height direction to the metal other than Li becomes 1.230, and the molar ratio B of Li in the filling in the lower half area to the metal other than Li becomes 1.255. At this time, the molar ratio B / molar ratio A is 1.02. In addition, a non-aqueous electrolyte secondary battery is made under the same conditions as in Example 1.
[0077] <Example 3>
[0078] The ratio of lithium hydroxide monohydrate filled on the bottom surface of the sintering container to the mixed powder M filled on the lithium hydroxide monohydrate is set to 0.01:100 in terms of mass conversion, and a filling is formed in the sintering container. The mixing ratio of Ni-Co-Al coprecipitated hydroxide and lithium hydroxide monohydrate in the mixed powder M is adjusted so that the molar ratio A of Li in the filling in the upper half area when the filling is divided into two equal parts in the height direction relative to the metal other than Li becomes 1.236, and the molar ratio B of Li in the filling in the lower half area relative to the metal other than Li becomes 1.248. At this time, the molar ratio B / molar ratio A is 1.01. In addition, a non-aqueous electrolyte secondary battery is prepared under the same conditions as in Example 1.
[0079] <Comparative Example 1>
[0080] Only the mixed powder M is filled in the sintering container to form a filler in the sintering container. The mixing ratio of lithium hydroxide monohydrate in the mixed powder M to the Ni-Co-Al coprecipitated hydroxide is adjusted so that the molar ratio B of Li to metals other than Li in each filler in the upper half region and the lower half region when the filler is divided into two equal parts in the height direction of the filler becomes 1.242. At this time, the molar ratio B / molar ratio A is 1. In addition, a non-aqueous electrolyte secondary battery is prepared under the same conditions as in Example 1.
[0081] <Comparative Example 2>
[0082] The ratio of lithium hydroxide monohydrate filled on the bottom surface of the calcining container to the mixed powder M filled on the lithium hydroxide monohydrate is set to 7:100 in terms of mass conversion, and a filling is formed in the calcining container. The mixing ratio of Ni-Co-Al coprecipitated hydroxide and lithium hydroxide monohydrate in the mixed powder M is adjusted so that the molar ratio A of Li in the filling to metals other than Li in the upper half of the area when the filling is divided into two equal parts in the height direction becomes 1.160, and the molar ratio B of Li in the filling to metals other than Li in the lower half of the area becomes 1.339. At this time, the molar ratio B / molar ratio A is 1.15. In addition, a non-aqueous electrolyte secondary battery is made under the same conditions as in Example 1.
[0083] [Determination of crystallite size]
[0084] The lithium nickel composite oxide obtained in each embodiment and each comparative example was taken from the vicinity of the top surface and the vicinity of the bottom surface of the calcining container, and the respective crystallite sizes were measured. Here, the crystallite size refers to the average size of the crystallite, and the crystallite refers to the region that can be regarded as a single crystal present in the primary particle. The X-ray diffraction device of Bruker AXS (strain) was used for high-precision measurement, and the obtained data was subjected to Rietveld analysis using DIFFRAC plusTOPAS to obtain the crystallite size.
[0085] The crystallite size variation was evaluated by subtracting the crystallite size of the lithium nickel composite oxide sampled from the bottom of the calcining container from the crystallite size of the lithium nickel composite oxide sampled from the top of the calcining container and using the absolute value of the difference according to the following criteria.
[0086] A: 0nm or more and less than 15nm
[0087] B: 15nm or more and less than 20nm
[0088] C: 20nm or more
[0089] C was evaluated as poor, B was evaluated as good, and A was evaluated as better.
[0090] [Discharge rate characteristics]
[0091] The non-aqueous electrolyte secondary battery of each embodiment and each comparative example is charged with a constant current at a current value of 0.2C until the voltage becomes 4.2V, and then charged with a constant voltage at 4.2V until the current becomes 0.02C. Then, discharge at a constant current at a current value of 0.2C until the voltage becomes 2.5V, and measure the discharge capacity of 0.2C. Next, charge at a constant current at a current value of 0.2C until the voltage becomes 4.2V, and then charge at a constant voltage at 4.2V until the current becomes 0.02C. Then, discharge at a constant current at a current value of 1.0C until the voltage becomes 2.5V, and measure the discharge capacity of 1.0C. Then, the discharge rate characteristic is obtained by the following formula.
[0092] Discharge rate characteristics = (0.2C discharge capacity / 1.0C discharge capacity) × 100
[0093] The obtained discharge rate characteristics were evaluated according to the following criteria.
[0094] A: More than 98.5%
[0095] B: 98.0% or more and less than 98.5%
[0096] C: less than 98.0%
[0097] C was evaluated as poor, B was evaluated as good, and A was evaluated as better.
[0098] Table 1 summarizes the variation in crystallite size and the evaluation results of discharge rate characteristics in each example and each comparative example.
[0099] [Table 1]
[0100] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 The molar ratio of the upper area is A 1.173 1.230 1.236 1.242 1.160 The molar ratio of the lower area is B 1.314 1.255 1.248 1.242 1.339 Mole ratio B / mole ratio A 1.12 1.02 1.01 1 1.15 Deviation of crystallite size A A B C C Discharge rate characteristics A A B C C
[0101] When the filling material filled in the sintering container is divided into two equal parts in the height direction, the molar ratio A of Li in the filling material to the metal other than Li in the upper half region and the molar ratio B of Li in the filling material to the metal other than Li in the lower half region satisfy 1<B / A<1.15. Compared with Comparative Examples 1 and 2 that do not satisfy 1<B / A<1.15, the deviation of the crystallite size is suppressed, and the discharge rate characteristics are also improved. In addition, among Examples 1 to 3, the deviation of the crystallite size is suppressed, and the discharge rate characteristics are also improved, compared with Example 3 that does not satisfy 1.02≤B / A≤1.12, which satisfies 1.02≤B / A≤1.12.
[0102] Description of Reference Numerals
[0103] 5, 5a, 5b filler, 7 calcination container, 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 case body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 bulging portion, 23 filter, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cover, 28 sealing gasket.
Claims
1. A method for producing a lithium nickel composite oxide, comprising the following steps: a filling step of filling a calcining container with a Ni-containing metal compound and a Li compound to obtain a filling containing the Ni-containing metal compound and the Li compound; and a firing step of firing the filling material filled in the firing container, When the filling filled in the calcining container in the filling step is divided into two equal parts in the height direction, the molar ratio A of Li in the filling to the metal other than Li in the upper half area and the molar ratio B of Li in the filling to the metal other than Li in the lower half area satisfy 1<B / A<1.
15.
2. The method for producing a lithium nickel composite oxide according to claim 1, wherein: The molar ratio A and the molar ratio B satisfy 1.02≤B / A≤1.
12.
3. The method for producing a lithium nickel composite oxide according to claim 1 or 2, wherein: The Li compound includes lithium hydroxide.