A micro-stress calculation method for transgranular stress corrosion crack initiation
Through electron backscattering diffraction images and Smit factor calculation normal and shear stress, the problem of difficult microscopic stress in the existing technology is solved, providing an accurate evaluation method for the occurrence of crystalline stress corrosion cracks, and improving material life Accuracy and ease of operation.
Patent Information
- Application Number
- CN202310106739.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-13
AI Technical Summary
The prior art is difficult to directly measure and calculate microscopic stress in metal materials, especially during the initiation of transcrystal stress corrosion cracks, and the lack of effective microscopic stress calculation methods leads to insufficient accuracy in the evaluation of material life.
A microscopic stress calculation method is adopted to record the microcrack position by electron backscattering diffraction image acquisition and scanning electron microscope. Combining Smit factor and Euler angle to calculate the normal and shear stress, the cumulative distribution probability curve is drawn, and the microscopic stress is analyzed. Type and level, threshold conditions are proposed to evaluate the invasion of transcrystalline stress corrosion cracks.
It provides a new method from a mechanical perspective to reflect the normal and shear stress levels on the slip plane intuitively and quantify, make up for the gap in microstress calculation of transcrystal stress corrosion cracking, reduce costs, improve operation ease and Applicability, suitable for a variety of materials and environments.
Smart Images

Figure CN116202869B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of stress corrosion crack initiation, and in particular relates to a micro stress calculation method for transgranular stress corrosion crack initiation. Background Art
[0002] Stress corrosion cracking is a common cause of failure of in-service equipment such as petrochemical and nuclear power. Stress corrosion failure can be divided into several parts, including microcrack initiation, microcrack growth and merging of cracks, and macro crack extension. For crack extension, most of the service life of defect construction is evaluated based on the perspective of fracture mechanics (stress intensity factor and J integral). However, for components with smooth surfaces, the crack initiation time occupies a major part of the service life. Therefore, crack initiation plays a vital role in stress corrosion cracking.
[0003] At present, there is still controversy over the evaluation of stress corrosion crack initiation and the factors affecting stress corrosion crack nucleation. From a mechanical point of view, stress corrosion cracks always tend to initiate at locations where stress and strain are concentrated. Stress corrosion cracking is closely related to stress levels. Generally, an increase in stress levels can accelerate the stress corrosion failure of materials, especially tensile stress that can cause plastic deformation of materials. Macro stress can be easily measured by load sensors. However, real metal materials are composed of a large number of grains (micrometer scale), and the macro stress level is only a reflection of the comprehensive mechanical properties of these grains, and cannot represent the stress level of a single grain or grain boundary. In fact, the initiation of cracks always originates in the grains or grain boundaries, and its nucleation law is closely related to the local stress level on the grains or grain boundaries. At present, there is no experimental technology that can directly measure microscopic stress.
[0004] EAWest and GSWAs from the University of Michigan proposed a method for calculating grain boundary stress based on Schmid factor correction. This method needs to consider the angle between the grain boundary plane and the loading direction and the slip initiation ability of adjacent grains at the same time. Although this method proposes a useful framework for calculating microscopic grain boundary stress, the angle between the grain boundary plane and the loading direction can only be measured by the destructive sample method of slicing (layer-by-layer grinding or focused ion beam cutting). In addition, this method is only applicable to the calculation of grain boundary stress, but not to the calculation of intragranular stress caused by transgranular crack initiation.
[0005] Transgranular stress corrosion cracking often occurs in metal materials with face-centered cubic structures, mainly because dislocation slip is easily activated for coordinated deformation. Therefore, transgranular stress corrosion cracks are always easy to nucleate on the dominant slip plane. The dominant slip system of austenite is {111}<1-10>. For a single grain, the ability to initiate slip is related to the Schmidt factor. The larger the value of the Schmidt factor, the higher the ability to initiate slip. For the slip-induced film rupture theory, the integrity of the passivation film or corrosion product is destroyed under the slip tearing force, and the fresh matrix surface exposed in the slip area is prone to rapid corrosion and dissolution. Under the repeated action of continuous slip, film rupture and dissolution, the crack nucleates on the slip plane and gradually grows into a macroscopic large crack, which finally leads to material failure. For this stress corrosion failure mechanism, the nucleation of the crack depends on the tearing force of the slip.
[0006] Therefore, establishing the relationship between local slip plane stress and crack initiation based on the perspective of micromechanics will provide a more accurate and effective method for evaluating the transgranular stress corrosion cracking life of metal materials. Summary of the invention
[0007] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for calculating micro stress of transgranular stress corrosion crack initiation.
[0008] The present invention solves the technical problem by the following technical solutions:
[0009] A method for calculating micro stress of transgranular stress corrosion crack initiation, characterized in that the steps of the method are:
[0010] S1, collect electron backscatter diffraction images of the sample surface;
[0011] S2. Perform stress corrosion crack initiation test on the sample and obtain microcracks that can be used for analysis. The length range of microcracks is 2 to 3 grains.
[0012] S3, using a scanning electron microscope to record the location of transgranular stress corrosion microcracks in the marked area and correspond it with the electron backscatter diffraction image;
[0013] S4. Calculate the stress value borne by the four covalent planes of the cracked grain's dominant slip plane, σ N is the normal stress, τ is the shear stress, and the calculation formula is as follows:
[0014]
[0015]
[0016] Where: σ is the applied tensile load;
[0017] m is the Schmidt factor value of the cracked grain;
[0018] m avg is the average Schmidt factor value of metal materials;
[0019] α is the angle between the normal to the slip plane and the tensile direction;
[0020] According to the solved α value, it is substituted into the calculation formula of normal stress and shear stress, the normal stress values and shear stress values of all microcracks are statistically analyzed, and the cumulative distribution probability curve of normal / shear stress value and number of cracked grains is plotted. The correlation between cracking and microstress type and level is analyzed, and the threshold condition is proposed.
[0021] Moreover, the angle α in step S4 is calculated by the Euler angle output by the electron backscatter diffraction image, and the calculation process is:
[0022] Obtaining the average Euler angle of cracked grains from electron backscatter diffraction images It is transformed from the sample coordinate system to the crystal coordinate system through the transformation matrix:
[0023]
[0024]
[0025]
[0026]
[0027] Where: ψ is the nutation angle;
[0028] θ is the precession angle;
[0029] is the rotation angle;
[0030] The transformation matrix of the average Euler angle of the cracked grain is By multiplying with the four covalent planes in the preferred slip plane (i.e., (111), (-111), (1-11), (11-1)), these slip planes can be located in the crystal coordinate system of the grain;
[0031] By performing vector dot multiplication of the slip plane corresponding to the cracked grain and the crystal coordinates of the tensile direction, and then removing their respective moduli, the cosine value of the angle between the normal of the slip plane and the tensile direction can be obtained. The angle α can be obtained by calculating through inverse trigonometric functions.
[0032] Moreover, the device used for the stress corrosion crack initiation test in step S2 includes a fixed block, a sliding block, a screw, a compression spring, a gasket, a nut and a fixed sliding rod. The sample is fixedly clamped between the fixed block and the sliding block by pins, and the middle part of the sample is placed in the corrosion groove. The rear end of the sliding block is provided with a threaded hole, and the screw is fixedly installed in the threaded hole. The screw is sequentially covered with a compression spring, a gasket and a nut. Through holes are symmetrically provided on both sides of the rear end of the sliding block, and the fixed sliding rod is inserted into the through holes.
[0033] The advantages and beneficial effects of the present invention are:
[0034] 1. From a mechanical point of view, the present invention proposes to use the microscopic stress on the slip plane as a basis for judging the initiation of transgranular stress corrosion cracking, providing a new idea and method for life assessment of transgranular stress corrosion cracking materials.
[0035] 2. The present invention reveals the relationship between the slip plane and the crystallographic properties of the grains and the external load through the force analysis of grain slip deformation, and proposes a stress calculation model during slip, which can intuitively and quantitatively respond to the normal and shear stress levels generated on the slip plane during grain deformation. This method fills the gap in micro-stress calculation of transgranular stress corrosion cracking.
[0036] 3. The present invention proposes a theoretical calculation method for the angle between the slip plane and the stretching direction with the help of electron backscatter diffraction image results. Compared with the method of obtaining by destroying the sample, it has low cost, simple operation, strong applicability, and will be more advantageous especially for the statistical calculation of large amounts of data.
[0037] 4. The present invention is not limited to a single material and medium environment, but can be extended to other transgranular stress corrosion cracking times caused by slip and tearing. It is an important means and method for evaluating stress corrosion crack initiation and stress corrosion life, and has important reference value for evaluating the structural integrity of metal materials in corrosive environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 is a flow chart of the present invention;
[0039] Figure 2 It is a schematic diagram of the device for stress corrosion crack initiation test of the present invention;
[0040] Figure 3 It is a schematic diagram of the force on the dominant slip plane when the grain is deformed in the present invention;
[0041] Figure 4 This is a diagram showing the normal / shear stress distribution of cracked and uncracked grains of the present invention.
[0042] Description of Reference Numerals
[0043] 1-fixed block, 2-pin, 3-corrosion groove, 4-sample, 5-sliding block, 6-screw, 7-compression spring, 8-washer, 9-nut, 10-fixed slide rod. DETAILED DESCRIPTION
[0044] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0045] This example takes the microscopic stress calculation of stress corrosion crack initiation of Monel 400 alloy, a material used for core parts of fluorine chemical industry, in a hydrofluoric acid vapor environment as an example. Figure 1 As shown;
[0046] (1) Grind and polish the Monel 400 alloy tensile specimen to obtain a high-quality surface;
[0047] (2) Use EBSD to capture and obtain crystallographic images of metal surfaces;
[0048] (3) Use a constant load stress corrosion test device to conduct stress corrosion crack initiation tests on the specimens, such as Figure 2 As shown, the device consists of a fixed block 1, a pin 2, a corrosion groove 3, a sample 4, a sliding block 5, a screw 6, a compression spring 7, a gasket 8, a nut 9 and a fixed sliding rod 10.
[0049] (3.1) The clamping sections at both ends of the sample 4 are fixed on the fixed block 1 and the sliding block 5 respectively by fixing pins. A threaded hole is turned on the rear of the sliding block 5, and the screw 6 is screwed into the thread of the sliding block. In addition, through holes are symmetrically set on both sides of the rear of the sliding block 5, and the fixed slide rod 10 is inserted to fix the sliding block 5 and the fixed block 1 and keep them horizontal. After the sample 4 and the sliding block 5 are fixed, the compression spring 7, the gasket 8 and the nut 9 are inserted into the screw 6 in turn. According to Hooke's law, the nut 9, the compression spring 7, and the sliding block 5 are moved horizontally with a wrench to apply a certain tensile load to the sample 4. According to the compression of the spring and the spring stiffness coefficient (152N / mm), the applied tensile load can be obtained. Therefore, the required deformation of the material can be determined according to the stress-strain curve of uniaxial tension, and the corresponding load can be achieved by adjusting the compression of the spring to achieve the purpose of loading deformation. In addition, the device can achieve load retention to ensure that the material will not experience stress relaxation during the subsequent corrosion process. In this article, a tensile stress of 250MPa is used for crack initiation test;
[0050] (3.2) The stress corrosion crack initiation test provides enough microcracks for later statistical analysis, so the crack length range is preferably around 2-3 grains. In this paper, the crack size is less than 150μm for calculation (the grain size of Monel 400 alloy is around 50μm).
[0051] (4) After the Monel 400 specimen was subjected to a stress corrosion test under a tensile stress of 250 MPa in hydrofluoric acid vapor for 12 hours, the specimen was taken out and the positions of all transgranular stress corrosion microcracks in the marked area were recorded using a scanning electron microscope and matched with the EBSD image;
[0052] (5) Establish a micro-stress calculation model for the initiation of transgranular stress corrosion cracks caused by slip plane tearing;
[0053] (5.1) Figure 3 As shown, the force state analysis on the slip plane when the crystal is deformed is given. The externally applied stress is:
[0054]
[0055] Where F is the load applied by the loading device, and A is the cross section of the specimen perpendicular to the loading direction. Assuming that the stress is evenly distributed inside the material, for the slip plane, the normal stress and shear stress on it are calculated as follows:
[0056]
[0057]
[0058] Where: F0 is the load borne by the slip plane, A0 is the area of the slip plane;
[0059] Furthermore, the deformation of slip is related to the Schmidt factor. Considering the ratio of the single grain and the average Schmidt factor of the material, the normal stress and shear stress on the slip plane are further corrected:
[0060]
[0061]
[0062] Where: σ is the applied tensile load;
[0063] m is the Schmidt factor value of the cracked grain;
[0064] m avg is the average Schmidt factor value of metal materials;
[0065] α is the angle between the normal to the dominant slip plane and the tensile direction;
[0066] (6) Through the above formula, the micro stress can be obtained according to the applied stress and the angle between the normal of the slip plane and the loading direction. The applied stress is known and only the α angle needs to be obtained. Since Monel 400 is a typical face-centered cubic structure material, its dominant slip system is {111}<1-10>. Therefore, the α angle is the angle between the normal of the {111} plane (including four covalent planes) and the loading direction. The present invention uses the Euler angle results collected in combination with EBSD to obtain the α angle through theoretical calculation. The specific steps are as follows:
[0067] (6.1) Calculate the stress values (normal stress and shear stress) borne by the four covalent planes of the cracked grain's dominant slip plane {111} using the following formula:
[0068]
[0069]
[0070] Where σ is the applied tensile load; m is the Schmidt factor value of the cracked grain; m avg is the average Schmidt factor value of the metal material; α is the angle between the normal direction of the dominant slip plane {111} and the tensile direction;
[0071] (6.2) The angle between the normal of the slip plane and the tensile direction is calculated by the Euler angle output by EBSD. The calculation idea is:
[0072] (6.2.1) Obtaining the average Euler angle of cracked grains from EBSD The sample coordinate system is converted to the crystal coordinate system through the conversion matrix. The specific calculation process is:
[0073]
[0074]
[0075]
[0076]
[0077] Where: ψ is the nutation angle;
[0078] θ is the precession angle;
[0079] is the rotation angle;
[0080] (6.2.2) The transformation matrix of the average Euler angle of the cracked grains By multiplying with the four covalent planes in the preferred slip plane {111} (i.e., (111), (-111), (1-11), (11-1)), these slip planes can be located in the crystal coordinate system of the grain;
[0081] (6.2.3) Perform vector dot multiplication of the slip plane {111} corresponding to the cracked grain and the crystal coordinates of the tensile direction, and then remove their respective moduli to obtain the cosine value of the angle between the normal of the slip plane {111} and the tensile direction. The angle α can be obtained by inverse trigonometric calculation;
[0082] (6.3) According to the solved α value, substitute it into the formula of normal stress and shear stress to calculate the corresponding value. Perform statistical analysis on the normal stress and shear stress values of all cracks, draw the cumulative distribution probability curve of normal / shear stress value and number of cracked grains, analyze the correlation between cracking and micro stress type and level, and propose threshold conditions for the evaluation criteria of stress corrosion crack initiation;
[0083] (7) Figure 4 The distribution of stress corrosion crack initiation and microscopic stress types and stress levels of Monel 400 alloy in hydrofluoric acid vapor environment is given. The statistical results include 56 cracked grains and 48 uncracked grains, a total of 104 grains were investigated. Figure 4 The results of (a) and (b) show that the probability distribution curve of transgranular stress corrosion cracking of Monel 400 in hydrofluoric acid vapor and normal stress in the (140MPa-155MPa) and (165MPa-190MPa) segments shifts to the right, which means that, under the same probability, higher stress is required to support crack initiation in these normal stress segments. However, there is no such rule in the (155MPa-165MPa) stress segment, which seems to mean that the normal stress and the initiation of transgranular cracks are not closely related.
[0084] In contrast, the shear stress has a stronger correlation, and the number of cracked grains at high stress values is higher than that of uncracked grains. It can also be seen from the cumulative distribution probability curve that the curve of cracked grains moves to the right as a whole, indicating that grain cracking occurs under high shear stress. It can be further concluded that the shear stress value required for the cracking of general grains is at least more than 116MPa, which can be used as the critical threshold for the initiation of transgranular stress corrosion cracking of Monel 400 alloy in a hydrofluoric acid vapor environment.
[0085] Therefore, from the perspective of mechanics, the present invention proposes to use micro stress as the basis for judging the initiation of transgranular stress corrosion cracking, and provides a new idea and method for the life assessment of stress corrosion cracking; through the force analysis on the grain scale of slip-induced transgranular cracking, the relationship between the slip plane and the crystallographic characteristics of the grain and the external load is revealed, and a stress calculation model during slip is proposed, which intuitively and quantitatively reflects the normal and shear stress levels generated on the slip plane when the grain is deformed. This method fills the gap in the calculation of micro stress of transgranular stress corrosion cracking. With the help of EBSD results, a theoretical calculation method for the angle between the slip plane and the tensile direction is proposed. Compared with the method of obtaining the sample by destroying it, it has low cost, simple operation, strong applicability, and will be more advantageous for the statistical calculation of a large amount of data; the micro stress calculation method for the initiation of transgranular stress corrosion cracking proposed by the present invention is not only limited to a single material and medium environment, but can be extended to other transgranular stress corrosion cracking times caused by slip tearing. It is an important means and method for evaluating the initiation of stress corrosion cracks and the life of stress corrosion, and has important reference value for the evaluation of the structural integrity of metal materials in corrosive environments.
[0086] Although the embodiments and drawings of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments and drawings.
Claims
1. A microscopic stress calculation method for transgranular stress corrosion crack initiation, characterized in that: The steps of the method are: S1, collect electron backscatter diffraction images of the sample surface; S2. Perform stress corrosion crack initiation test on the sample and obtain microcracks that can be used for analysis. The length range of microcracks is 2 to 3 grains. S3, using a scanning electron microscope to record the location of transgranular stress corrosion microcracks in the marked area and correspond it with the electron backscatter diffraction image; S4. Calculate the stress value borne by the four covalent planes of the cracked grain's dominant slip plane, σ N is the normal stress, τ is the shear stress, and the calculation formula is as follows: Where: σ is the applied tensile load; m is the Schmidt factor value of the cracked grain; m avg is the average Schmidt factor value of metal materials; α is the angle between the normal to the slip plane and the tensile direction; According to the solved α value, it is substituted into the calculation formula of normal stress and shear stress, and the normal stress values and shear stress values of all microcracks are statistically analyzed and the cumulative distribution probability curve of normal / shear stress value and number of cracked grains is drawn. The correlation between cracking and micro stress type and level is analyzed, and the threshold condition is proposed; The angle α in step S4 is calculated by the Euler angle output by the electron backscatter diffraction image, and the calculation process is: Obtaining the average Euler angle of cracked grains from electron backscatter diffraction images It is transformed from the sample coordinate system to the crystal coordinate system through the transformation matrix: Where: ψ is the nutation angle; θ is the precession angle; is the rotation angle; The transformation matrix of the average Euler angle of the cracked grain is By multiplying with the four covalent planes in the preferred slip plane (i.e., (111), (-111), (1-11), (11-1)), these slip planes can be located in the crystal coordinate system of the grain; By performing vector dot multiplication of the slip plane corresponding to the cracked grain and the crystal coordinates of the tensile direction, and then removing their respective moduli, the cosine value of the angle between the normal of the slip plane and the tensile direction can be obtained. The angle α can be obtained by calculating through inverse trigonometric functions.
2. The micro-stress calculation method for transgranular stress corrosion crack initiation according to claim 1 is characterized in that: The device used for the stress corrosion crack initiation test in step S2 includes a fixed block, a sliding block, a screw, a compression spring, a gasket, a nut and a fixed sliding rod. The sample is fixedly clamped between the fixed block and the sliding block by pins, and the middle part of the sample is placed in the corrosion groove. The rear end of the sliding block is provided with a threaded hole, and the screw is fixedly installed in the threaded hole. The screw is sequentially covered with a compression spring, a gasket and a nut. Through holes are symmetrically provided on both sides of the rear end of the sliding block, and the fixed sliding rod is inserted into the through holes.