A method for preparing catalytic cracking catalyst
By combining magnesium source, silicon source and rare earth compounds, spraying into microspheres, and hydrothermal crystallization and exchange modification, the problem of insufficient pore structure of the catalyst is solved, significantly improving the pore structure and activity of the catalyst, and improving heavy oil Conversion and resistance to heavy metals.
Patent Information
- Application Number
- CN202111467601.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-03
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-12-03
AI Technical Summary
When the catalytic cracking catalyst is prepared by in-situ crystallization in the prior art, the pore structure of the catalyst is insufficient and the pore penetration is poor, which affects its activity and heavy oil conversion ability.
After mixing the magnesium source solution with the silicon source solution, rare earth compounds are added, and then sprayed into microspheres after beating. After roasting, hydrothermal crystallization is carried out with sodium silicate, guide agent and alkali solution. Then, it is modified by exchange of ammonia water and boric acid. Finally, Further exchange was performed using ammonium salts to prepare a catalyst with developed pore structure.
The pore structure and activity of the catalyst are significantly improved, the specific surface area and medium-large pore volume are increased, the heavy oil conversion ability and heavy metal resistance are improved, the coke by-products are reduced, and the total liquid collection and conversion rate are improved.
Smart Images

Figure BDA0003392197960000221 
Figure BDA0003392197960000222 
Figure BDA0003392197960000223
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysts, and in particular relates to a method for preparing a catalytic cracking catalyst. Background Art
[0002] The rich and developed pore structure of catalytic cracking catalyst is one of the important directions of catalyst design. For heavy oil catalytic cracking reaction, the unobstructed pores of catalyst can not only enhance the mass transfer and diffusion performance and improve the catalytic efficiency, but also make it easy to remove hydrocarbons between particles during stripping in the catalytic cracking unit, greatly reducing the amount of hydrocarbons entrained by the catalyst into the regenerator, which is conducive to the recovery of catalyst activity after regeneration and improving the actual operation activity and selectivity of the unit. Therefore, the development of FCC catalysts with good pore structure, good molecular sieve stability and small crystals has always been an important direction to improve the efficiency of catalytic cracking.
[0003] Among catalytic cracking catalysts, there is a process that uses in-situ crystallization to prepare catalysts. This catalyst uses kaolin as the main raw material. After being spray-formed into microspheres, the matrix and active components are simultaneously generated under alkaline hydrothermal conditions. Then, after being modified, a catalyst with high active component content and good synergy with the matrix can be prepared. This catalyst can be used alone in a catalytic cracking unit or in combination, and the product distribution of the unit can be flexibly adjusted. Compared with traditional bonded catalysts, its unique synthesis process has unique advantages such as good pore structure, high activity stability, small molecular sieve grains, and strong heavy oil conversion ability. As the proportion of slag blending in the unit becomes higher and higher, the requirements for catalyst performance are also higher. The catalyst should not only have a good heavy oil conversion ability, but also have excellent coke selectivity. Therefore, the design of the acidity and pore structure of the highly active in-situ crystallization catalyst is very important.In order to improve the pore structure, enhance the heavy oil conversion capacity, improve the activity, and reduce the further conversion of intermediate distillates and naphtha, CN108097329A mentions the use of amorphous silicon magnesium materials as carrier materials to improve the carrier pore structure; CN101636227A proposes the use of solid powder of silicon dioxide with a large specific surface area added to the system as a carrier material to improve the catalyst pore structure; CN101745373A introduces a catalyst preparation method containing two aluminum oxide matrix materials with stepped pore distribution; C N1978593B reported a catalytic cracking catalyst characterized in that the catalyst contains a mesoporous material with a pseudo-boehmite structure, and the mesoporous material contains aluminum oxide, silicon oxide and metal oxides, such as rare earth oxide; CN1322917C reported a mesoporous silicon-aluminum material and a preparation method thereof, and CN201910155755.1 introduced a petroleum cracking catalyst and a preparation method thereof, wherein amorphous silicon-magnesium colloid was used in the preparation of the carrier material; CN201811226378.8 introduced in detail a Preparation of hydrocracking catalyst, which mentions the use of silicon-magnesium carrier to load metal, CN107497481A, CN107497481B mainly describe a method for preparing silicon-magnesium zeolite, first prepare a magnesium sulfate solution A of a certain concentration, then prepare a silicon-containing solution B of a certain concentration, mix the two, and introduce an organic template to perform hydrothermal crystallization at 150-180°C for 10-48h to obtain silicon-magnesium zeolite raw powder; CN201910467181.1 adds 4 to pseudo-boehmite in the preparation of sulfur transfer agent % polyacrylamide to improve the pores; CN109207192A uses methyl cellulose, activated carbon, polyvinyl alcohol, urea, sodium polyacrylate, polyacrylic acid, ammonium polyacrylate, preferably sodium polyacrylate as a pore expander; CN111073684 uses starch as a matrix pore expander for producing clean gasoline catalysts; CN110496611 mentions that when preparing alumina carriers, one or more of polyvinyl alcohol, sodium polyacrylate, starch, carbon black and crop stem shell powder are added as pore expanders. CN200810143378.1 uses one or two of sepiolite, kaolin and roasted kaolin to prepare Mg-Y type zeolite, which has a good pore structure; CN200910084253.0 introduces a method for increasing the specific surface area of diatomite, but the article does not mention how to use these methods to prepare Y type zeolite with good pore structure. Through the analysis of the above patents, whether in hydrocracking catalysts, sulfur transfer or catalytic cracking catalysts, the improvement of catalyst pores is generally achieved by soft and hard template methods. The soft template has the disadvantage of environmental problems caused by the subsequent roasting and removal of organic matter. The hard template method uses carbon powder or other inorganic materials to adjust the pore structure by controlling the appropriate addition amount, but it has the disadvantages of disordered pore structure, difficult to control pore volume, and difficult to control catalyst strength.There are also some pore expansion technologies that use chemical silicon oxide formed after thermal conversion of kaolin and then extracted in an alkaline system to form pores, or rely on the stacking gaps between kaolin particles or add organic matter and heat it to increase the porosity. From a technical point of view, there are shortcomings such as complex procedures, environmental pollution or poor strength. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a catalytic cracking catalyst to solve the problems of insufficient pore structure of the catalyst, pore penetration, and changes in the growth micro-areas of active components when the catalytic cracking catalyst is prepared by in-situ crystallization in the prior art.
[0005] To achieve the above object, the present invention provides a method for preparing a catalytic cracking catalyst, comprising the following steps:
[0006] (1) adding a magnesium source solution to a silicon source solution, mixing them evenly to obtain a silicon-magnesium material, and then adding a rare earth compound, aging, to obtain a rare earth-containing silicon-magnesium material;
[0007] (2) mixing the rare earth-containing silicon-magnesium material with kaolin, a dispersant and / or a reinforcing agent and deionized water, beating the mixture, spraying the mixture into microspheres, calcining the mixture, and then mixing the mixture with sodium silicate, a directing agent, an alkaline solution and water, and crystallizing the mixture to obtain a crystallized product;
[0008] (3) exchanging and modifying the crystallized product with ammonia water and boric acid, and then calcining to obtain a primary calcined material;
[0009] (4) exchanging the primary calcined material with ammonium salt and / or rare earth, and obtaining a catalyst after calcination.
[0010] The method for preparing the catalyst cracking catalyst of the present invention comprises dissolving a magnesium source into a magnesium source solution at a liquid-to-solid mass ratio of 2 to 10.
[0011] The method for preparing the catalyst cracking catalyst of the present invention comprises the following steps: in step (1), the pH of the silicon-magnesium material is adjusted to 8-14 before adding the rare earth compound.
[0012] The method for preparing a catalytic cracking catalyst of the present invention, wherein the aging condition in step (1) is aging treatment at 50-80°C for 10-240 minutes, the aging temperature is preferably 50-75°C, and the aging treatment time is preferably 30-180 minutes.
[0013] The method for preparing a catalytic cracking catalyst of the present invention, wherein the rare earth compound in step (1) is calculated as oxide RE2O3, the mass ratio of RE2O3 to silicon-magnesium material is 0.1-10:100, and the molar ratio of Si:Mg in the silicon-magnesium material is 0.1-10.
[0014] The method for preparing a catalyst cracking catalyst of the present invention, wherein the silicon source in step (1) is one or more of water glass, silica sol and white carbon black; the magnesium source is one or more of magnesium chloride, magnesium nitrate and magnesium sulfate; and the rare earth compound is one or more of rare earth nitrate, rare earth chloride and rare earth carbonate.
[0015] The method for preparing a catalyst cracking catalyst of the present invention, wherein in step (2), the mass ratio of the rare earth-containing silicon-magnesium material to kaolin is 0.1-20:100, the mass ratio of the dispersant to kaolin is 1-20:100, preferably 1-15:100, the mass ratio of the reinforcing agent to kaolin is 1-20:100, preferably 2-8:100, and the solid content of the slurry after mixing and beating is 30-50%.
[0016] In the method for preparing a catalytic cracking catalyst of the present invention, the particle size of the microspheres obtained by spraying in step (2) is 20 to 110 μm.
[0017] The method for preparing the catalyst cracking catalyst of the present invention, wherein the calcination temperature in step (2) is 600-1000° C., the calcination time is 1-3 hours, and the crystallization conditions are 85-95° C. for 16-36 hours.
[0018] Specifically, in step (2), when the microspheres are calcined, they can be calcined at 600-850°C for 1-3 hours to obtain low-temperature calcined microspheres, or calcined at 860-1000°C for 1-3 hours to obtain high-temperature calcined microspheres, or a mixture of low-temperature calcined microspheres and high-temperature calcined microspheres. After crystallization, the mother liquor is filtered out, and the filter cake is washed with deionized water until the pH is below 10.5, and dried to obtain a crystallized product with good pore structure and anti-wear performance and containing 20-60% NaY molecular sieve.
[0019] The preparation method of the catalyst cracking catalyst of the present invention, wherein the dispersant is sodium silicate and / or sodium pyrophosphate, the reinforcing agent is silica sol and / or alumina sol, the order of adding the dispersant and the reinforcing agent is not limited, and they can be added simultaneously or in batches.
[0020] The method for preparing a catalytic cracking catalyst of the present invention, wherein the kaolin in step (2) is one or more of soft kaolin, hard kaolinite and coal gangue, wherein the median diameter is 1.5 to 3.0 μm, the crystal kaolinite content is higher than 80%, the iron oxide content is lower than 1.7%, and the sum of the sodium oxide and the potassium oxide content is lower than 0.5%.
[0021] In the method for preparing a catalytic cracking catalyst of the present invention, the concentration of aqueous ammonia in step (3) is 5-25%, and the mass ratio of aqueous ammonia to crystallized product is 1:1.5-10.
[0022] In the method for preparing a catalytic cracking catalyst of the present invention, the mass ratio of the boron element to the crystallized product in step (3) is 0.01-0.20:1.
[0023] Specifically, the process of step (3) is that the crystallized product is first treated with ammonia water at 20-60° C. for 30-120 min, and the product after the ammonia water exchange is then exchanged with boric acid. The exchange process conditions are: pH 3-6, temperature 80-95° C., time 15-120 min; roasting temperature 500-950° C., time 0.5-2 hours, water vapor amount 0-100%. The exchange modification of ammonia water and boric acid can change the exchange order, that is, boric acid can be placed first and ammonia water can be placed later, or ammonia water can be placed first and boric acid can be placed later, without special limitation.
[0024] The method for preparing a catalytic cracking catalyst of the present invention, wherein the ammonium salt in step (4) is one or more of ammonium sulfate, ammonium chloride, ammonium nitrate and ammonium phosphate, preferably ammonium chloride and / or ammonium nitrate, and the rare earth is one or more of rare earth chloride, rare earth nitrate and rare earth hydroxide, preferably rare earth chloride and / or rare earth nitrate.
[0025] The method for preparing the catalyst cracking catalyst of the present invention comprises: taking the mass of the catalyst as 100%, the catalyst contains 20-60% of NaY molecular sieve, the content of Na2O is less than or equal to 0.4%, and the specific surface area is 200-500m 2 / g, pore volume 0.40~0.55mL / g.
[0026] There is no particular restriction on the composition of the directing agent in the present invention. A common directing agent can be used. For example, the directing agent composition in Example 1 of CN1232862A is prepared. The molar ratio of the directing agent recommended by the present invention is: (14-16)SiO2: (0.7-1.3)Al2O3: (14-16)Na2O: (300-330)H2O.
[0027] The present invention discloses a preparation method for improving the pore structure of a catalytic cracking catalyst, which mainly uses kaolin as a raw material, adds deionized water, a dispersant and / or a reinforcing agent, a silicon-magnesium material, and a rare earth material, and mixes and slurries the mixture, and sprays the mixture into microspheres; the sprayed microspheres are calcined, and the calcined microspheres are mixed with a directing agent, water glass, and sodium hydroxide, and a crystallization reaction is carried out under hydrothermal conditions to obtain a crystallized product with a good pore structure and containing 20 to 60% NaY molecular sieve. The product after crystallization is then exchanged with ammonia water, boric acid, ammonium salt, and rare earth to prepare a catalytic cracking catalyst with a developed pore structure. The invention is characterized in that the sprayed microspheres contain silicon-magnesium materials, kaolin, a dispersant, rare earth elements, and the like. The introduced silicon-magnesium material can have a rich pore structure and a high specific surface area depending on the preparation conditions, and form a cross-linked structure inside the microsphere precursor. After modification with rare earth elements, on the one hand, the interwoven structure of the microspheres is further significantly changed. On the other hand, the addition of rare earth elements changes the micro-region environment of the microsphere precursor, which can provide more sufficient space and environment for the growth of molecular sieves. It can also combine with the silicon-magnesium material to form a tighter organizational structure, essentially improving the pore structure of the microsphere precursor. The prepared catalyst has a richer and more developed pore structure, and the structure is not easy to change.
[0028] The beneficial effects of the present invention are:
[0029] The invention includes silicon-magnesium materials, kaolin, dispersants, rare earth elements, etc. in the spray microspheres. The introduced silicon-magnesium materials can have rich pore structures and high specific surface areas according to different preparation conditions, and form a cross-linked structure inside the microsphere precursor. After modification with rare earth elements, on the one hand, the interwoven structure of the microspheres is further significantly changed. On the other hand, the addition of rare earth elements changes the micro-region environment of the microsphere precursor, which can provide more sufficient space and environment for the growth of molecular sieves. It can also be combined with silicon-magnesium materials to form a tighter organizational structure, which essentially improves the pore structure of the microsphere precursor. The prepared catalyst has a richer and more developed pore structure, and the structure is not easy to change. Therefore, compared with the traditional technical solution, the specific surface area of the crystallized product has increased by 30m 2 / g or above, the total pore volume increases, and mainly the volume of medium and large pores increases.
[0030] On the one hand, rare earth-modified silicon-magnesium materials are introduced in the spray pulping stage, so that the pore structure of the intermediate product is more developed and the molecular sieve content is higher; on the other hand, in the post-modification stage, the exchange modification of ammonia water and boric acid is used to effectively clean up the polymers such as silicon aluminum adhering to the surface of the intermediate product after crystallization, and further make the pores penetrated; in addition, the introduction of boron, combined with rare earth modification, can further enhance the heavy oil conversion and heavy metal resistance of the catalyst. Therefore, this patent designs an in-situ crystallization catalyst with a more developed pore structure and outstanding performance from the construction of the catalyst pore structure, the adjustment of acidity and the introduction of functional components. Therefore, under the same heavy oil yield conditions, the coke by-product of the catalyst is reduced by 0.89 percentage points and the total liquid yield is increased by 1.05 percentage points; under the same heavy metal pollution conditions, the conversion rate is increased by 0.99 percentage points, and the heavy metal resistance is significantly enhanced. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is the N2 adsorption / desorption isotherm of the catalyst in Example 1 of the present invention;
[0032] Figure 2 This is the N2 adsorption / desorption isotherm of Comparative Example 2. DETAILED DESCRIPTION
[0033] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.
[0034] Source of raw materials:
[0035] Kaolin: industrial product, sourced from Lanzhou Petrochemical Company Catalyst Factory
[0036] Magnesium chloride: chemically pure, Sinopharm Chemical Reagent Co., Ltd.
[0037] Sodium silicate solution: industrial product, collected from the catalyst plant of Lanzhou Petrochemical Company, (SiO2: 19.75%, Na2O:
[0038] 6.95%, H2O:73.30%)
[0039] Alkaline silica sol: industrial product, Yantai Hengxin Chemical Technology Co., Ltd., (SiO2: 30%)
[0040] Directing agent: industrial agent, collected from the catalyst plant of Lanzhou Petrochemical Company, proportion:
[0041] 16SiO2:Al2O3:15Na2O:320H2O
[0042] NaOH solution: industrial product, obtained from the catalyst plant of Lanzhou Petrochemical Company (NaOH: 24%)
[0043] Sodium pyrophosphate: analytical grade, Tianjin Kemeiou Chemical Reagent Co., Ltd.
[0044] Alumina sol: industrial product, sourced from Lanzhou Petrochemical Company Catalyst Plant (Al2O3: 21.22%)
[0045] Hydrochloric acid: chemically pure
[0046] Ammonia: Chemically pure
[0047] Boric acid: chemically pure
[0048] Ammonium nitrate: chemically pure
[0049] Ammonium chloride: chemically pure
[0050] Ammonium sulfate, chemically pure
[0051] Specific analysis method:
[0052] The crystallinity of NaY molecular sieve was tested on a D / max-3C X-ray powder diffractometer manufactured by Rigaku Corporation of Japan, using X-ray diffraction to determine the crystallinity of the sample, and the method standard is Q / SYLS0596~2002. The silicon-aluminum ratio of NaY molecular sieve was tested using X-ray powder diffraction, and the method standard is Q / SYLS0573~2002. The sample pore distribution test used the Autosorb~3B specific surface measuring instrument of Quantachrome Company of the United States, and the specific surface area, pore size distribution and pore volume of the sample were determined by the N2 low temperature (77.3K) adsorption-desorption experimental method. Reaction performance evaluation: The catalyst cracking reaction selectivity was evaluated in the ACE catalytic cracking evaluation unit in the United States. The catalyst was pre-treated at 800°C and 100% water vapor for 17 hours.
[0053] Example 1
[0054] 10g of magnesium chloride was dissolved in 80mL of distilled water, and the dissolved solution was slowly injected into 242ml of sodium silicate solution and mixed for 30 minutes to obtain silicon-magnesium material with a final pH value of 13.2. Lanthanum nitrate rare earth was then added, and the lanthanum oxide / silicon-magnesium material in the lanthanum nitrate was 7.8% (mass ratio). The material after adding the rare earth was aged at 50°C for 4h. 200g of the aged material, 2000g of kaolin (calcined base), 40g of sodium silicate solution, 400g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 46%, which was spray-dried to obtain 1300g of spray microspheres P1 with a particle size of 20 to 110μm. A portion of the P1 spray soil ball was calcined at 925°C for 2.7 hours to obtain calcined microspheres G1, and the other portion was calcined at 650°C for 2.5 hours to obtain calcined microspheres B1. Then, 200g G1 and 300g B1 were mixed and sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water were added. The mixture was hydrothermally crystallized at 95°C for 30 hours, the mother liquor was filtered out, the mixture was washed with water until the pH was below 10.5, and the product J1 was obtained by drying.
[0055] 400 g of product J1 was added into a stainless steel kettle with stirring. At room temperature, 25% ammonia solution was added with a liquid-to-solid ratio of 8 and the treatment was carried out for 100 min. The washed material was filtered and exchanged with boric acid. The exchange process conditions were: pH 3.5, temperature 90°C, B: exchange material (dry basis) = 0.20 (mass ratio). After 100 min, the material was roasted at 500°C and 100% water vapor for 2 hours to obtain a roasted material. Ammonium chloride, ammonium sulfate and deionized water were added to the first roasted material, with ammonium chloride / the first roasted material = 0.2 (mass ratio) and ammonium sulfate / the first roasted material = 0.1 (mass ratio), and the mixture was exchanged at pH = 3.0-3.5 and 90°C for 40 minutes. The filtrate was filtered out, and the filter cake was washed with deionized water and dried to obtain the second roasted material; the second roasted material was calcined at 560°C and a water vapor introduction rate of 95% for 2 hours to obtain the second roasted material; the second roasted material was exchanged once with 0.8 mol / L hydrochloric acid, and the exchange conditions were: pH = 3.5, temperature was 90°C, and the treatment time was 1 hour. The exchanged material was filtered, washed, and dried to obtain a catalyst C-1 with a Na2O content of 0.58%.
[0056] Example 2
[0057] Dissolve 150g of magnesium nitrate in 320mL of distilled water, slowly inject the dissolved solution into 101g of alkaline silica sol solution, mix for 50 minutes, and finally pH value is 8.1 to obtain silicon magnesium material, then add cerium chloride rare earth, cerium oxide / silicon magnesium material in cerium chloride = 2.3% (mass ratio), the material after adding rare earth is aged at 80°C for 20min, 80g of aged material, 400g of kaolin (calcined base), 24g of sodium pyrophosphate, 4g of aluminum sol, and deionized water are prepared into a mixed slurry with a solid content of 32%, spray dried to obtain 300g of spray microspheres P2 with a particle size of 20 to 110μm. The P2 spray soil ball is roasted at 990°C for 1.5h to obtain the roasted microspheres G2. 100 g of G2 was added to sodium silicate solution, directing agent, sodium hydroxide solution and deionized water, and hydrothermally crystallized at 85° C. for 16 h. The mother liquor was filtered out, and the product was washed with water until the pH was below 10.5 and dried to obtain product J2.
[0058] 100 g of product J2 was added into a stainless steel kettle with stirring, and boric acid was used for exchange. The exchange process conditions were: pH 4.5, temperature 95°C, B: exchange material (dry basis) = 0.13 (mass ratio). After 40 minutes, it was filtered and washed, and then a 10% ammonia solution was added at 20°C with a liquid-to-solid ratio of 8. The treatment lasted for 100 minutes, and then the material was calcined at 700°C and 80% water vapor for 0.5 hours to obtain a calcined material. The calcined material is exchanged with ammonium nitrate and deionized water, with ammonium nitrate / calcined material = 0.3 (mass ratio), and the exchange is carried out at pH = 4.0-4.5 and 93°C for 1.5 hours. The filtrate is filtered to remove the filtrate, and the filter cake is washed with deionized water and dried to obtain an exchange material; the exchange material is calcined at 680°C for 2 hours to obtain a second calcined material; the second calcined material is exchanged once with rare earth chloride, and the exchange conditions are: cerium oxide in cerium chloride / second calcined material = 0.085 (mass ratio), pH = 3.5-4.2, temperature is 89°C, and time is 1 hour. The exchanged material is then exchanged with 3 mol / L sulfuric acid, and the exchange conditions are: pH = 3.8, temperature is 80°C, and treatment time is 30 minutes. After filtering, washing and drying, a catalyst C-2 with a Na2O content of 0.45% is obtained.
[0059] Example 3
[0060] Dissolve 50g of magnesium sulfate in 220mL of distilled water, dissolve 229g of white carbon black in 500ml of distilled water to form a turbid solution, slowly inject the magnesium sulfate solution into the white carbon black solution, mix for 60 minutes, obtain silicon magnesium material, the final pH value is 8.0, then add yttrium carbonate, yttrium oxide in yttrium carbonate / silicon magnesium material = 0.7% (mass ratio), the material after adding rare earth is aged at 70°C for 60min, and the aged material 100g, kaolin 700g (calcined base), sodium silicate 42g, aluminum sol 105g, deionized water are prepared into a mixed slurry with a solid content of 40%, spray dried, and 600g of spray microspheres P3 with a particle size of 20-110μm are obtained. The P3 spray soil ball is roasted at 990°C for 1.5h to obtain the roasted microsphere G3. 100 g of G3 was added to sodium silicate solution, directing agent, sodium hydroxide solution and deionized water, and hydrothermally crystallized at 85° C. for 16 h. The mother liquor was filtered out, and the product was washed with water until the pH was below 10.5 and dried to obtain product J3.
[0061] 70 g of the prepared crystallized product J3 was added to a stainless steel kettle under stirring, and a 5% ammonia solution was added at 40°C with a liquid-to-solid ratio of 10. The treatment was carried out for 120 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 5.8, temperature 92°C, B: exchange material (dry basis) = 0.18 (mass ratio). After 45 min, the material was calcined at 900°C for 0.5 hour to obtain a calcined material. The calcined material is exchanged with 5 mol / L sulfuric acid and deionized water, the exchange conditions are: pH = 4.0, temperature is 85 ° C, and the treatment time is 45 min. The exchanged material is exchanged with lanthanum carbonate, and the lanthanum oxide in the lanthanum carbonate / exchange material = 0.05 (mass ratio). The exchange is carried out at pH = 4.0-4.5 and 93 ° C for 0.5 hour, and the filtrate is filtered to remove the filtrate. The filter cake is washed with deionized water and dried to obtain the exchange material; the exchange material is then exchanged with ammonium sulfate, and the exchange conditions are: ammonium sulfate / exchange material = 0.20 (mass ratio), pH = 3.7-4.0, and temperature The exchange material is calcined at 660°C and a water vapor introduction rate of 50% for 2 hours to obtain a second roasted material; the second roasted material is exchanged once with 5 mol / L hydrochloric acid, and the exchange conditions are: pH = 3.3, temperature is 80°C, and the treatment time is 30 min. The exchange material is filtered, washed, and dried to obtain an exchange material; the exchange material is calcined at 600°C and a water vapor introduction rate of 100% for 2 hours to obtain a catalyst C-3 with a Na2O content of 0.52%.
[0062] Example 4
[0063] 80g of magnesium carbonate was dissolved in 260mL of distilled water, and the dissolved magnesium carbonate solution was slowly added to 648g of alkaline silica sol and mixed for 60 minutes to obtain a silicon-magnesium material with a final pH value of 10.3. Cerium nitrate was then added, and the cerium oxide / silicon-magnesium material in the cerium nitrate was 1.4% (mass ratio). The material after adding rare earth was aged at 70°C for 60min. 100g of the aged material, 700g of kaolin (calcined base), 42g of sodium silicate, 105g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 47%, which was spray-dried to obtain 600g of spray microspheres P4 with a particle size of 20 to 110μm. A portion of P4 was calcined at 1000°C for 1.5 h to obtain calcined microspheres G4, and the other portion was calcined at 800°C for 2 h to obtain calcined microspheres B4. Then, 800 g of G4 and 200 g of B4 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 89°C for 30 h. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J4.
[0064] 700 g of the crystallized product J4 was added into a stainless steel kettle under stirring, and an 8% ammonia solution was added at 60° C. with a liquid-to-solid ratio of 1.5. The mixture was treated for 50 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 3.9, temperature 88° C., B: exchange material (dry basis) = 0.12 (mass ratio). After 120 min, the material was calcined at 600° C. and 50% water vapor for 1 hour to obtain a calcined material. 9.9 mol / L nitric acid and deionized water were added to the calcined material. The exchange conditions were as follows: pH = 4.2, temperature was 40°C, and treatment time was 1 h. The exchanged material was exchanged with ammonium sulfate, ammonium sulfate / exchange product = 0.40 (mass ratio). The exchange was carried out at pH = 3.0-3.5 and 90°C for 1 hour. The filtrate was filtered out, and the filter cake was washed with deionized water and dried to obtain a second exchange material. The second exchange material was calcined at 500°C and a water vapor introduction rate of 85% for 2 hours to obtain a second roasted material. The second roasted material was exchanged once with 3 mol / L phosphoric acid. The exchange conditions were as follows: pH = 3.8, temperature was 90°C, and time was 1 hour. The exchanged material was filtered, washed, and dried to obtain a catalytic material C-4 with a Na2O content of 0.52%.
[0065] Example 5
[0066] 30g of magnesium nitrate was dissolved in 160ml of distilled water, and 83g of white carbon black was gradually dissolved in 200ml of distilled water to form a turbid solution. The dissolved magnesium nitrate solution was slowly added to the white carbon black turbid solution and mixed for 30 minutes to obtain a silicon-magnesium material with a final pH value of 9.3. Lanthanum chloride was then added, and the lanthanum oxide / silicon-magnesium material in the lanthanum chloride was 3.7% (mass ratio). The material after adding rare earth was aged at 50°C for 240min. 100g of the aged material, 589g of kaolin (calcined base), 76g of sodium silicate, 76g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 43%, which was spray-dried to obtain 600g of spray microspheres P5 with a particle size of 20 to 110μm. A portion of P5 was calcined at 970°C for 2.3 hours to obtain calcined microspheres G5, and the other portion was calcined at 850°C for 1.9 hours to obtain calcined microspheres B5. Then 200g of G5 and 200g of B5 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 87°C for 16 hours. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J5.
[0067] 320 g of the crystallized product J5 was added to a stainless steel kettle under stirring, and boric acid was used for exchange. The exchange process conditions were: pH 3.6, temperature 85°C, B: exchange material (dry basis) = 0.01 (mass ratio), filtered and washed after 15 minutes, and then a 15% ammonia solution was added at 40°C with a liquid-to-solid ratio of 4, and the treatment was carried out for 80 minutes. Then the material was calcined at 800°C for 1.5 hours to obtain a calcined material. Cerium nitrate and deionized water are added to the calcined material, and the exchange conditions are: cerium oxide in cerium nitrate / calcined material = 0.09 (mass ratio), pH = 3.6, temperature is 34°C, and processing time is 1 hour. The exchanged material is exchanged with ammonium chloride, ammonium chloride / exchange material = 0.20 (mass ratio), and exchanged at pH = 3.0-3.5 and 90°C for 1 hour. The filtrate is filtered to remove the filtrate, and the filter cake is washed with deionized water and dried to obtain an exchange material; the exchange material is calcined at 500°C and a water vapor introduction rate of 85% for 2 hours to obtain a second roasted material; the second roasted material is exchanged with sulfuric acid once again, and the exchange conditions are: pH = 3.2, temperature is 90°C, and time is 1 hour. The exchanged material is filtered, washed, and dried to obtain a catalytic material C-5 with a Na2O content of 0.42%.
[0068] Example 6
[0069] 100g of magnesium sulfate was dissolved in 500mL of distilled water, and the dissolved solution was slowly added to 675ml of water glass solution and mixed for 70 minutes to obtain a silicon-magnesium material with a final pH value of 12.3. Lanthanum carbonate was then added, and the lanthanum oxide / silicon-magnesium material in the lanthanum carbonate was 4.8% (mass ratio). The material after adding rare earth was aged at 60°C for 180min. 200g of the aged material, 4000g of kaolin (calcined base), 360g of sodium pyrophosphate, 360g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 38%, which was spray-dried to obtain 3500g of spray microspheres P6 with a particle size of 20 to 110μm.
[0070] A portion of P6 was calcined at 960°C for 1.4 hours to obtain calcined microspheres G6, and the other portion was calcined at 880°C for 2 hours to obtain calcined microspheres B6. Then 600g of G6 and 400g of B6 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 34 hours. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J6.
[0071] 820 g of the crystallized product J6 was added into a stainless steel kettle with stirring, and boric acid was used for exchange. The exchange process conditions were: pH 4.0, temperature 93°C, B: exchange material (dry basis) = 0.05 (mass ratio), filtered and washed after 60 minutes, and then a 20% ammonia solution was added at 60°C with a liquid-to-solid ratio of 7, and the treatment was carried out for 90 minutes. Then, the material was calcined at 650°C and 30% water vapor for 1.5 hours to obtain a calcined material. Ammonium sulfate and deionized water were added to the calcined material, and the exchange conditions were: ammonium sulfate / calcined material = 0.30 (mass ratio), pH = 3.6, temperature 34°C, and processing time 1h. The exchanged material was exchanged with ammonium chloride, ammonium chloride / calcined material = 0.20 (mass ratio), and exchanged at pH = 3.0-3.5 and 90°C for 1 hour. The filtrate was filtered out, and the filter cake was washed with deionized water and dried to obtain an exchange material; the exchange material was roasted at 500°C and a water vapor introduction rate of 85% for 2 hours to obtain a second roasted material; the second roasted material was exchanged with sulfuric acid again, and the exchange conditions were: pH = 3.2, temperature 90°C, and time for 1 hour. The exchanged material was filtered, washed, and dried to obtain a catalytic material C-6 with a Na2O content of 0.42%.
[0072] Example 7
[0073] 70g of magnesium chloride was dissolved in 300mL of distilled water, and the dissolved solution was slowly added to 604g of alkaline silica sol solution and mixed for 55 minutes to obtain a silicon-magnesium material with a final pH value of 11.5. Cerium nitrate was then added, and the cerium oxide / silicon-magnesium material in the cerium nitrate was 9.2% (mass ratio). The material after adding rare earth was aged at 75°C for 200min. 500g of the aged material, 5556g of kaolin (calcined base), 167g of sodium silicate, 167g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 36%, which was spray-dried to obtain 5500g of spray microspheres P7 with a particle size of 20 to 110μm. Part of P7 was calcined at 850°C for 2.3h to obtain calcined microspheres G7, and the other part was calcined at 680°C for 2.6h to obtain calcined microspheres B7. Then 750g of G7 and 250g of B7 were added to sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 32h. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J7.
[0074] 450 g of crystallized product J7 was added to a stainless steel kettle under stirring, and a 23% ammonia solution was added at 20°C with a liquid-to-solid ratio of 3. The mixture was treated for 40 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 4.2, temperature 95°C, B: exchange material (dry basis) = 0.09 (mass ratio). After 90 min, the material was calcined at 750°C and 60% water vapor for 0.5 hour to obtain a calcined material. The calcined material is exchanged with 4 mol / L hydrochloric acid, ammonium chloride and deionized water, with ammonium chloride / calcined material = 0.15 (mass ratio), and the exchange is carried out at pH = 4.0-4.5 and 93°C for 1.5 hours, and the filtrate is filtered to remove the filtrate, and the filter cake is washed with deionized water and dried to obtain the exchange material; the exchange material is roasted at 680°C for 2 hours to obtain the second roasted material; the second roasted material is exchanged with lanthanum chloride once again, and the exchange conditions are: lanthanum oxide in lanthanum chloride / second roasted material = 0.05 (mass ratio), pH = 3.5-4.2, temperature is 89°C, and time is 1 hour. The exchanged material is filtered, washed, and dried to obtain a catalytic material C-7 with a Na2O content of 0.39%.
[0075] Example 8
[0076] 130g of magnesium nitrate was dissolved in 400mL of distilled water, and the dissolved solution was slowly added to 947ml of sodium silicate solution and mixed for 25 minutes to obtain a silicon-magnesium material with a final pH value of 10.5. Cerium chloride was then added, and the cerium oxide / silicon-magnesium material in the cerium chloride was 11% (mass ratio). The material after adding rare earth was aged at 75°C for 100min. 120g of the aged material, 1091g of kaolin (calcined base), 76g of sodium silicate, 76g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 42%, which was spray-dried to obtain 750g of spray microspheres P8 with a particle size of 20 to 110μm. P8 was calcined at 630°C for 2.1h to obtain calcined microspheres B8, and then 800g of B8 was added to sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 94°C for 36h. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J8.
[0077] 250g of crystallized product J8 was added into a stainless steel kettle under stirring, and exchanged with boric acid. The exchange process conditions were as follows: pH 3.7, temperature 90°C, B: exchange material (dry basis) = 0.15 (mass ratio), filtered and washed after 30 minutes. 18% ammonia solution was added at 30°C, with a liquid-to-solid ratio of 5, and treated for 60 minutes. Then the material was roasted at 750°C and 60% water vapor for 0.5 hours to obtain a roasted material. The calcined material is exchanged with ammonium sulfate and deionized water, with ammonium sulfate / calcined material = 0.50 (mass ratio), and the exchange is carried out at pH = 4.0-4.5 and 93°C for 1.5 hours, the filtrate is filtered to remove the filtrate, and the filter cake is washed with deionized water and dried to obtain the exchange material; the exchange material is roasted at 660°C for 2 hours to obtain the second roasted material; the second roasted material is exchanged with cerium sulfate once again, and the exchange conditions are: cerium oxide in cerium sulfate / second roasted material = 0.05 (mass ratio), pH = 3.5-4.2, temperature is 89°C, and time is 1 hour. The exchanged material is then exchanged with 12 mol / L nitric acid, and the exchange conditions are: 60°C, pH = 3.0-3.5, and the treatment is carried out for 50 minutes. After filtering, washing and drying, a catalytic material C-8 with a Na2O content of 0.39% is obtained.
[0078] Example 9
[0079] 200g of magnesium nitrate was dissolved in 700mL of distilled water, and 1173g of white carbon black was gradually dissolved in 1000ml of distilled water to form a turbid solution. The dissolved magnesium nitrate solution was slowly added to the white carbon black turbid solution and mixed for 90 minutes to obtain a silicon-magnesium material with a final pH value of 7.3. Yttrium carbonate was then added, and the yttrium oxide / silicon-magnesium material in the yttrium carbonate was 6.6% (mass ratio). The material after adding rare earth was aged at 50°C for 220min. 120g of the aged material, 857g of kaolin (calcined base), 137g of sodium pyrophosphate, 154g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 42%, which was spray-dried to obtain 750g of spray microspheres P9 with a particle size of 20 to 110μm. A portion of P9 was calcined at 890°C for 1.5 h to obtain calcined microspheres G9, and the other portion was calcined at 770°C for 1.8 h to obtain calcined microspheres B9. Then 200 g of G9 and 400 g of B9 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 88°C for 28 h. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J9.
[0080] 550 g of crystallized product J9 was added into a stainless steel kettle with stirring, and a 6% ammonia solution was added at 50°C with a liquid-to-solid ratio of 9. The mixture was treated for 50 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 3.9, temperature 89°C, B: exchange material (dry basis) = 0.03 (mass ratio). After 15 min, the material was calcined at 880°C and 20% water vapor for 0.5 hour to obtain a calcined material. 14.5 mol / L sulfuric acid, ammonium sulfate and deionized water were added to the calcined material for exchange, with ammonium sulfate / calcined material = 0.40 (mass ratio), and the exchange was carried out at pH = 3.3-3.9 and 90° C. for 1 hour, and the filtrate was filtered out, and the filter cake was washed with deionized water to obtain an exchange material; the exchange material was calcined at 500° C. and a water vapor introduction rate of 85% for 2 hours to obtain a second roasted material; the second roasted material was exchanged once with cerium chloride, and the exchange conditions were: cerium oxide in cerium chloride / second roasted material = 0.02 (mass ratio), pH = 3.5-4.2, temperature of 90° C., and time of 1 hour. The exchanged material was filtered, washed, and dried to obtain a catalytic material C-9 with a Na2O content of 0.57%.
[0081] Example 10
[0082] 90g of magnesium chloride was dissolved in 200mL of distilled water, and the dissolved solution was slowly added to 246g of alkaline silica sol solution and mixed for 70 minutes to obtain a silicon-magnesium material with a final pH value of 8.5. Cerium nitrate was then added, and the cerium oxide / silicon-magnesium material in the cerium nitrate was 5.7% (mass ratio). The material after adding rare earth was aged at 70°C for 170min. 500g of the aged material, 2631g of kaolin (calcined base), 105g of sodium pyrophosphate, 395g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 36%, which was spray-dried to obtain 2100g of spray microspheres P10 with a particle size of 20 to 110μm. A portion of P10 was calcined at 830°C for 2.8 hours to obtain calcined microspheres G10, and the other portion was calcined at 670°C for 3.6 hours to obtain calcined microspheres B10. Then, 900g G10 and 300g B10 were added to sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 32 hours. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J10.
[0083] 550 g of the crystallized product J10 was added to a stainless steel kettle under stirring, and boric acid was used for exchange. The exchange process conditions were: pH 3.5, temperature 86°C, B: exchange material (dry basis) = 0.07 (mass ratio). After 120 minutes, 13% ammonia solution was added at 50°C, the liquid-to-solid ratio was 5.5, and the treatment was carried out for 70 minutes. After filtering and washing, the material was calcined at 600°C and 70% water vapor for 2 hours to obtain a calcined material. The calcined material is exchanged with lanthanum sulfate and deionized water, with lanthanum oxide in lanthanum sulfate / calcined material = 0.06 (mass ratio), and the exchange is carried out at pH = 4.0-4.5 and 93°C for 1.5 hours, the filtrate is filtered to remove the filtrate, and the filter cake is washed with deionized water to obtain the exchange material; the exchange material is calcined at 700°C for 2 hours under the condition of a water vapor introduction amount of 25% to obtain a second calcined material; the second calcined material is exchanged once with ammonium chloride, and the exchange conditions are: ammonium chloride / second calcined material = 0.16 (mass ratio), pH = 3.5-4.2, temperature is 86°C, and time is 1 hour. The exchanged material is then treated with 6 mol / L nitric acid at 50°C and pH = 4.0-4.5 for 1 hour, and the catalytic material C-10 with a Na2O content of 0.28% is obtained after filtering, washing and drying.
[0084] Comparative Example 1
[0085] Compared with Example 3, 229g of white carbon black was dissolved in 500ml of distilled water to form a turbid solution, and then yttrium carbonate was added, and the yttrium oxide / white carbon black in the yttrium carbonate was 0.7% (mass ratio). The material after adding rare earth was aged at 70°C for 60min, and 100g of the aged material, 700g of kaolin (calcined base), 42g of sodium silicate, 105g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 40%, and spray-dried to obtain 600g of spray microspheres P11 with a particle size of 20 to 110μm. The P11 spray soil ball was calcined at 990°C for 1.5h to obtain calcined microspheres G11. 100g of G11 was added to sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 85°C for 16h, and the mother liquor was filtered to remove it, and it was washed with water until the pH was below 10.5 and dried to obtain product J11.
[0086] 70 g of the crystallized product J11 was added to a stainless steel kettle under stirring, and a 5% ammonia solution was added at 40°C with a liquid-to-solid ratio of 10. The mixture was treated for 120 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 5.8, temperature 92°C, B: exchange material (dry basis) = 0.18 (mass ratio). After 45 min, the material was calcined at 900°C for 0.5 hour to obtain a calcined material. The calcined material is exchanged with 5 mol / L sulfuric acid and deionized water, the exchange conditions are: pH = 4.0, temperature is 85 ° C, and the treatment time is 45 min. The exchanged material is exchanged with lanthanum carbonate, and the lanthanum oxide in the lanthanum carbonate / exchange material = 0.05 (mass ratio). The exchange is carried out at pH = 4.0-4.5 and 93 ° C for 0.5 hour, and the filtrate is filtered to remove the filtrate. The filter cake is washed with deionized water and dried to obtain the exchange material; the exchange material is then exchanged with ammonium sulfate, and the exchange conditions are: ammonium sulfate / exchange material = 0.20 (mass ratio), pH = 3.7-4.0, and temperature The temperature is 91°C and the time is 0.5 hour. The exchanged material is filtered, washed and dried to obtain an exchange material; the exchange material is roasted at 660°C and a water vapor introduction amount of 50% for 2 hours to obtain a second roasted material; the second roasted material is exchanged once with 5mol / L hydrochloric acid, and the exchange conditions are: pH=3.3, temperature is 80°C, and the treatment time is 30min. The exchanged material is filtered, washed and dried to obtain an exchange material; the exchange material is roasted at 600°C and a water vapor introduction amount of 100% for 2 hours to obtain a catalyst C-11 with a Na2O content of 0.52%.
[0087] Comparative Example 2
[0088] Compared with Example 1, 10g of magnesium chloride was dissolved in 80mL of distilled water, and the dissolved solution was added to lanthanum nitrate rare earth, lanthanum oxide / magnesium chloride in lanthanum nitrate = 7.8% (mass ratio), and the material after adding rare earth was aged at 50°C for 4h. 200g of the aged material, 2000g of kaolin (calcined base), 40g of sodium silicate solution, 400g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 46%, and spray-dried to obtain 1300g of spray microspheres P12 with a particle size of 20 to 110μm. Part of the P12 spray soil ball was calcined at 925°C for 2.7 hours to obtain calcined microspheres G12, and the other part was calcined at 650°C for 2.5 hours to obtain calcined microspheres B12. Then, 200g G12 and 300g B12 were mixed and added with sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water. The mixture was hydrothermally crystallized at 95°C for 30 hours, the mother liquor was filtered out, the mixture was washed with water until the pH was below 10.5, and the product J12 was obtained by drying.
[0089] 400 g of product J12 was added to a stainless steel kettle under stirring. At room temperature, 25% ammonia solution was added with a liquid-to-solid ratio of 8. The mixture was treated for 100 min. The washed mixture was filtered and exchanged with boric acid. The exchange process conditions were: pH 3.5, temperature 90°C, B: exchange material (dry basis) = 0.20 (mass ratio). After 100 min, the material was roasted at 500°C and 100% water vapor for 2 hours to obtain a roasted material. Ammonium chloride, ammonium sulfate and deionized water were added to the first roasted material, with ammonium chloride / the first roasted material = 0.2 (mass ratio) and ammonium sulfate / the first roasted material = 0.1 (mass ratio), and the mixture was exchanged at pH = 3.0-3.5 and 90°C for 40 minutes. The filtrate was filtered out, and the filter cake was washed with deionized water and dried to obtain the first roasted material; the first roasted material was roasted at 560°C and a water vapor introduction rate of 95% for 2 hours to obtain the second roasted material; the second roasted material was exchanged once with 0.8 mol / L hydrochloric acid, and the exchange conditions were: pH = 3.5, temperature was 90°C, and the treatment time was 1 hour. The exchanged material was filtered, washed, and dried to obtain the catalyst C-12 with a Na2O content of 0.58%.
[0090] Comparative Example 3
[0091] Compared with Example 7, 70g of magnesium chloride was dissolved in 300mL of distilled water, and the dissolved solution was slowly added to 604g of alkaline silica sol solution, mixed for 55 minutes, and the final pH value was 11.5. The material was aged at 75°C for 200min. 500g of the aged material, 5556g of kaolin (burning base), 167g of sodium silicate, 167g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 36%, spray dried, and 5500g of spray microspheres P13 with a particle size of 20 to 110μm were obtained. A portion of P13 was calcined at 850°C for 2.3 h to obtain calcined microspheres G13, and the other portion was calcined at 680°C for 2.6 h to obtain calcined microspheres B13. Then, 750 g of G13 and 250 g of B13 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 32 h. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J13.
[0092] 450 g of the crystallized product J13 was added to a stainless steel kettle under stirring, and a 23% ammonia solution was added at 20°C with a liquid-to-solid ratio of 3. The mixture was treated for 40 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 4.2, temperature 95°C, B: exchange material (dry basis) = 0.09 (mass ratio). After 90 min, the material was calcined at 750°C and 60% water vapor for 0.5 hour to obtain a calcined material. The calcined material is exchanged with 4 mol / L hydrochloric acid, ammonium chloride and deionized water, with ammonium chloride / first calcined material = 0.15 (mass ratio), and the exchange is carried out at pH = 4.0-4.5 and 93°C for 1.5 hours. The filtrate is filtered to remove the filtrate, and the filter cake is washed with deionized water and dried to obtain an exchange material; the exchange material is calcined at 680°C for 2 hours to obtain a second calcined material; the second calcined material is exchanged once with lanthanum chloride, and the exchange conditions are: lanthanum oxide in lanthanum chloride / second calcined material = 0.05 (mass ratio), pH = 3.5-3.8, temperature is 89°C, and time is 1 hour. The exchanged material is filtered, washed, and dried to obtain a catalyst C-13 with a Na2O content of 0.39%.
[0093] Comparative Example 4
[0094] Compared with Example 5, 30g of magnesium nitrate was dissolved in 160mL of distilled water, 83g of white carbon was gradually dissolved in 200ml of distilled water to form a turbid solution, the dissolved magnesium nitrate solution was slowly added to the white carbon turbid solution, mixed for 30 minutes, and a silicon-magnesium material was obtained, the final pH value was 9.3, and lanthanum chloride rare earth was added, wherein lanthanum oxide / silicon-magnesium material = 3.7% (mass ratio), the material after adding rare earth was aged at 50°C for 240min, and 100g of the aged material, 589g of kaolin (burning base), 76g of sodium silicate, 76g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 43%, spray dried, and 600g of spray microspheres P14 with a particle size of 20 to 110μm were obtained. A portion of P14 was calcined at 970°C for 2.3 hours to obtain calcined microspheres G14, and the other portion was calcined at 850°C for 1.9 hours to obtain calcined microspheres B14. Then 200g of G14 and 200g of B14 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 87°C for 16 hours. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J14.
[0095] 320 g of the crystallized product J14 was added to a stainless steel kettle under stirring, and cerium nitrate and deionized water were added. The exchange conditions were: cerium oxide in cerium nitrate / calcined material = 0.09 (mass ratio), pH = 3.6, temperature was 34°C, and treatment time was 1 hour. The exchanged material was exchanged with ammonium chloride, ammonium chloride / exchange material = 0.20 (mass ratio), and exchanged at pH = 3.0-3.5 and 90°C for 1 hour. The filtrate was filtered to remove the filtrate, and the filter cake was washed with deionized water and dried to obtain an exchange material; the exchange material was calcined at 500°C and a water vapor introduction rate of 85% for 2 hours to obtain a second roasted material; the second roasted material was exchanged once with sulfuric acid, and the exchange conditions were: pH = 3.2, temperature was 90°C, and time was 1 hour. The exchanged material was filtered, washed, and dried to obtain a catalytic material C-14 with a Na2O content of 0.47%.
[0096] Comparative Example 5
[0097] Compared with Example 10, 90g of magnesium chloride was dissolved in 200mL of distilled water, and the dissolved solution was slowly added to 246g of alkaline silica sol solution and mixed for 70 minutes to obtain a silicon-magnesium material with a final pH of 8.5. After aging at 70°C for 170min, cerium nitrate was added, wherein the cerium oxide / silicon-magnesium material of the cerium nitrate was 5.7% (mass ratio). 500g of the material after rare earth, 2631g of kaolin (burning base), 105g of sodium pyrophosphate, 395g of alkaline silica sol and deionized water were added to prepare a mixed slurry with a solid content of 36%, which was spray-dried to obtain 2100g of spray microspheres P15 with a particle size of 20 to 110μm. A portion of P15 was calcined at 830°C for 2.8 hours to obtain calcined microspheres G15, and the other portion was calcined at 670°C for 3.6 hours to obtain calcined microspheres B15. Then, 900g of G15 and 300g of B15 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 32 hours. The mother liquor was filtered to remove the mother liquor, and the product was washed with water until the pH was below 10.5 and dried to obtain product J15.
[0098] 550 g of product J15 was added into a stainless steel kettle with stirring, and boric acid was used for exchange. The exchange process conditions were: pH 3.5, temperature 86°C, B: exchange material (dry basis) = 0.07 (mass ratio). After 120 minutes, 13% ammonia solution was added at 50°C, the liquid-to-solid ratio was 5.5, and the treatment was carried out for 70 minutes. After filtering and washing, the material was roasted at 600°C and 70% water vapor for 2 hours to obtain a roasted material. The calcined material is exchanged with lanthanum sulfate and deionized water, with lanthanum oxide in lanthanum sulfate / calcined material = 0.06 (mass ratio), and the exchange is carried out at pH = 4.0-4.5 and 93°C for 1.5 hours, the filtrate is filtered to remove the filtrate, and the filter cake is washed with deionized water to obtain the exchange material; the exchange material is calcined at 700°C for 2 hours under the condition of a water vapor introduction amount of 25% to obtain a second calcined material; the second calcined material is exchanged once with ammonium chloride, and the exchange conditions are: ammonium chloride / second calcined material = 0.16 (mass ratio), pH = 3.5-4.2, temperature is 86°C, and time is 1 hour. The exchanged material is then treated with 6 mol / L nitric acid at 50°C and pH = 4.0-4.5 for 1 hour, and the catalytic material C-15 with a Na2O content of 0.27% is obtained after filtering, washing and drying.
[0099] Table 1 In-situ crystallization process conditions and preparation results
[0100]
[0101] Table 2 Pore structure characteristics of crystallized products
[0102]
[0103] Table 3 Reaction performance of catalysts ACE evaluation
[0104]
[0105]
[0106] Table 4 Reaction performance of catalyst (ACE evaluation under 5000V, 3000Ni pollution conditions)
[0107]
[0108] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a catalytic cracking catalyst, characterized in that: The following steps are involved: (1) adding a magnesium source solution to a silicon source solution, mixing them evenly to obtain a silicon-magnesium material, and then adding a rare earth compound, aging, to obtain a rare earth-containing silicon-magnesium material; (2) mixing the rare earth-containing silicon-magnesium material with kaolin, a dispersant and / or a reinforcing agent and deionized water, beating the mixture, spraying the mixture into microspheres, calcining the mixture, and then mixing the mixture with sodium silicate, a directing agent, an alkaline solution and water, and crystallizing the mixture to obtain a crystallized product; (3) exchanging and modifying the crystallized product with ammonia water and boric acid, and then calcining to obtain a primary calcined material; (4) The primary calcined material is exchanged with ammonium salt and / or rare earth, and the catalyst is obtained after calcination.
2. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The magnesium source is dissolved into a magnesium source solution at a liquid-to-solid mass ratio of 2 to 10.
3. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (1), the pH of the silicon-magnesium material is adjusted to 8-14 before adding the rare earth compound.
4. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The aging condition in step (1) is aging treatment at 50-80° C. for 10-240 minutes.
5. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The aging condition in step (1) is aging treatment at 50-75° C. for 30-180 minutes.
6. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (1), the rare earth compound is calculated as oxide RE2O3, the mass ratio of RE2O3 to silicon-magnesium material is 0.1-10:100, and the molar ratio of Si:Mg in the silicon-magnesium material is 0.1-10.
7. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (1), the silicon source is one or more of water glass, silica sol and white carbon black; the magnesium source is one or more of magnesium chloride, magnesium nitrate and magnesium sulfate; and the rare earth compound is one or more of rare earth nitrate, rare earth chloride and rare earth carbonate.
8. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (2), the mass ratio of the rare earth-containing silicon-magnesium material to kaolin is 0.1-20:100, the mass ratio of the dispersant to kaolin is 1-20:100, the mass ratio of the reinforcing agent to kaolin is 1-20:100, and the solid content of the slurry after mixing and beating is 30-50%.
9. The method for preparing a catalytic cracking catalyst according to claim 8, characterized in that: In step (2), the mass ratio of the dispersant to kaolin is 1-15:100, and the mass ratio of the reinforcing agent to kaolin is 2-8:
100.
10. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The particle size of the microspheres obtained by spraying in step (2) is 20-110 μm.
11. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (2), the calcination temperature is 600-1000° C., the calcination time is 1-3 h, and the crystallization conditions are 85-95° C. for 16-36 h.
12. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The dispersant is sodium silicate and / or sodium pyrophosphate; the reinforcing agent is silica sol and / or aluminum sol.
13. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (2), the kaolin is one or more of soft kaolin and hard kaolinite, with a median diameter of 1.5-3.0 μm, a crystal kaolinite content higher than 80%, iron oxide lower than 1.7%, and a sum of sodium oxide and potassium oxide lower than 0.5%.
14. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (3), the concentration of aqueous ammonia is 5-25%, and the mass ratio of aqueous ammonia to the crystallized product is 1:1.5-10.
15. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (3), the mass ratio of boron element to crystallized product is 0.01-0.20:
1.
16. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The process of step (3) is that the crystallized product is first treated with ammonia water at 20-60° C. for 30-120 min, and the product exchanged with ammonia water is then exchanged with boric acid. The exchange process conditions are: pH 3-6, temperature 80-95° C., time 15-120 min; roasting temperature 500-950° C., time 0.5-2 hours, water vapor amount 0-100%.
17. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (4), the ammonium salt is one or more of ammonium sulfate, ammonium chloride, ammonium nitrate and ammonium phosphate, and the rare earth is one or more of rare earth chloride, rare earth nitrate and rare earth hydroxide.
18. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step (4), the ammonium salt is ammonium chloride and / or ammonium nitrate, and the rare earth is rare earth chloride and / or rare earth nitrate.
19. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: Based on the catalyst mass as 100%, the catalyst contains 20-60% NaY molecular sieve, the Na2O content is less than or equal to 0.4%, and the specific surface area is 200-500 m 2 / g, pore volume 0.40~0.55mL / g.