FeCo / C catalytic materials, FeCo / C working electrodes and electrochemical sensors
Through the synthesis of FeCo/C catalytic materials and the combination of electrochemical sensors, the cumbersome catalyst synthesis and the shortcomings of traditional monitoring methods in advanced oxidation technology are solved, efficient catalysis of PMS and real-time monitoring of organic pollutants are achieved, and the degradation efficiency and Detection accuracy.
Patent Information
- Application Number
- CN202310155133.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-23
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-02-23
AI Technical Summary
In the existing technology, the catalyst synthesis steps for activating PMS in advanced oxidation technologies (AOPs) are cumbersome and energy-intensive, and the traditional organic polluted wastewater monitoring methods have cumbersome processing procedures, high operational requirements, and high costs, which are not conducive to real-time monitoring.
FeCo/C catalytic material is used, synthesized through a one-step method of FeCo-ZIFs and polyacrylonitrile (PAN) to form a porous carbon support, exposing the active sites of iron-cobalt alloy, used to catalyze the degradation of PMS, and combined with electrochemical sensors to realize organic pollutants real-time monitoring.
It achieves high catalytic activity of PMS and efficient and stable degradation of organic pollutants, simplifies the preparation process of catalytic materials, reduces energy consumption, and realizes real-time monitoring of the degradation progress of organic matter in water through electrochemical sensors, improving detection sensitivity and accuracy.
Smart Images

Figure CN116212875B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a FeCo / C catalytic material and also to a FeCo / C working electrode and an electrochemical sensor based on the catalytic material. Background Art
[0002] In recent years, advanced oxidation processes (AOPs) using peroxymonosulfate (PMS) as an activator have attracted extensive attention from researchers at home and abroad. Existing catalysts that activate PMS have great potential in the field of AOPs. For example, Cai et al. 3 O 4 Encapsulated in MOFs, it was applied to catalyze the degradation of 4-chlorophenol by PMS and showed excellent degradation performance (Environ. Sci. Technol., 2015, 49, 2350-7). However, this method has complicated synthesis steps, requires high-temperature hydrothermal treatment, and has high energy consumption.
[0003] Traditional methods for monitoring organic polluted wastewater include high performance liquid chromatography (HPLC), spectroscopy, etc. These methods have the following disadvantages: (1) the treatment process is cumbersome; (2) high requirements for operators; (3) large precision instruments are expensive and difficult to maintain, which is not conducive to real-time monitoring of pollutant degradation. In recent years, electrochemical analysis has been widely used in analysis, medicine and other fields due to its convenience, high sensitivity and high degree of automation. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a FeCo / C catalytic material, which has a stable structure and the metal active sites on the carrier are fully exposed, thereby effectively improving its catalytic activity to PMS; also provided are a FeCo / C working electrode and an electrochemical sensor based on the above catalytic material, which can enable the catalytic material to degrade organic matter while also monitoring the degradation process of organic pollutants in water in real time.
[0005] Technical solution: The FeCo / C catalytic material of the present invention is prepared by the following method, which specifically comprises the following steps:
[0006] (1) dissolving 2-methylimidazole (HMIM) in N,N-dimethylformamide (DMF) to obtain solution A; dissolving a divalent cobalt salt and a trivalent iron salt in DMF to obtain solution B;
[0007] (2) adding solution B to solution A, and FeCo-ZIFs are rapidly formed in the reaction solution; after the reaction is complete, adding polyacrylonitrile (PAN) thereto, stirring and dissolving, to form a mixed solution of FeCo-ZIFs and PAN; using DMF as a solvent, synthesizing the FeCo-ZIFs structure in one step, and using FeCo-ZIFs as a precursor of metal active sites, which can make the active sites of the iron-cobalt alloy on the support after calcination more fully exposed;
[0008] (3) applying the obtained mixed solution on the fibrous material and placing it in an oven for drying, so that the liquid phase PAN is converted into a solid phase PAN film, and the FeCo-ZIFs are fixed on the fibrous material through the PAN film;
[0009] (4) The dried material is placed in an inert atmosphere and calcined at high temperature. After calcination, the fibrous material forms porous carbon, and the FeCo-ZIFs supported on the porous carbon are converted into FeCo alloy after high-temperature annealing, and the FeCo / C catalytic material is obtained after grinding.
[0010] Wherein, in step (1), in solution A, the mass concentration of 2-methylimidazole is 0.175 g / mL; in solution B, the mass concentration of the metal salt is 1 g / mL; the divalent cobalt salt is Co(NO 3 ) 2 ; The ferric iron salt is Fe(NO 3 ) 3 ;Co(NO 3 ) 2 With Fe(NO 3 ) 3 The mass ratio is 4 to 5:1.
[0011] Wherein, in step (2), the mixing volume ratio of solution A to solution B is 1.5-2:1; the reaction time of FeCo-ZIFs is 15-25 min; the mass volume ratio of PAN to the reaction solution is 0.06-0.1 g:1 mL, and the dissolution time is 20-30 min.
[0012] Wherein, in step (3), the fibrous material is any one of paper, cotton, dyed cloth or nylon; the drying temperature is 50 to 80° C., and the drying time is 60 to 72 hours.
[0013] Wherein, in step (4), the calcination temperature is 700-1000° C., the calcination time is 6-14 hours, and after cooling to room temperature, it is left to stand for 2-5 hours before being taken out to prevent spontaneous combustion after contact with air.
[0014] The FeCo / C working electrode based on the above FeCo / C catalytic material is prepared by the following method, which specifically includes the following steps:
[0015] (1) dispersing FeCo / C catalytic material in N-methylpyrrolidone (NMP), and then adding polyvinylidene fluoride (PVDF) thereto to obtain FeCo / C turbid solution;
[0016] (2) Apply FeCo / C turbid liquid to the filling part on one side of the graphite electrode plate, apply it evenly and then dry it; after it is fully dried, turn over the graphite electrode plate and apply it to the filling part on the other side of the graphite electrode plate, apply it and then dry it to obtain a FeCo / C working electrode.
[0017] Wherein, in step (1), the mass volume ratio of FeCo / C catalytic material to NMP is 0.09-0.1 g:1 mL; the mass ratio of FeCo / C catalytic material to PVDF is 9-10:1.
[0018] Wherein, in step (2), the area of the coated portion of the graphite electrode plate accounts for 10-80% of the area of the entire electrode plate, the turbid liquid is dripped onto the coated portion of the electrode plate, and drained with a rubber-tipped dropper to make it evenly dispersed in the coated portion; the mass area ratio of the FeCo / C catalytic material to the coated portion is 10-15 mg: 1 cm 2 , that is, the mass concentration of FeCo / C catalyst material loaded on the graphite electrode plate is 10-15 mg / cm 2 .
[0019] Wherein, in step (2), the drying temperature is 50-80° C. and the drying time is 8-12 h.
[0020] The electrochemical sensor based on the above-mentioned FeCo / C working electrode is composed of a FeCo / C working electrode, a graphite electrode and a coulometric analyzer. The two electrodes are connected in series with the coulometric analyzer through a wire. When in use, the FeCo / C working electrode and the graphite electrode are immersed in an organic pollutant solution. The FeCo / C working electrode, the graphite electrode, the organic pollutant solution and the coulometric analyzer form a closed loop through the wire.
[0021] Based on Faraday's law (Q = zFξ, F is the Faraday constant), the FeCo / C working electrode is used as the negative electrode and the graphite rod is used as the positive electrode, and they are immersed in the electrolyte solution containing organic pollutants. After adding PMS, the FeCo / C working electrode quickly undergoes redox reaction with PMS, and the generated active oxygen species act on the organic pollutants to degrade them efficiently. The working principle of the sensor is that a large amount of electron transfer occurs during the catalytic degradation of pollutants. The real-time charge obtained during the monitoring process is fitted with the pollutant concentration, and the degradation of organic pollutants and the progress of their reaction can be determined simultaneously.
[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The FeCo / C catalytic material of the present invention has high catalytic activity for PMS. When the initial concentration of bisphenol A is 10 ppm and the concentration of PMS is 0.50 g / L, Na 2 SO 4 Under the conditions of a concentration of 0.1 M and a temperature of 298 K, the degradation efficiency of bisphenol A of the FeCo / C working electrode containing the FeCo / C catalytic material reaches 98.02% within 10 minutes, achieving efficient and stable degradation of organic pollutants. At the same time, since the FeCo / C catalytic material is made into a FeCo / C electrode, it is beneficial to the recovery of the FeCo / C catalytic material; (2) The electrochemical sensor made of the FeCo / C catalytic material of the present invention realizes the efficient degradation of organic matter in saline wastewater and the real-time monitoring of the progress of organic matter degradation in water. Compared with traditional equipment, the volume of the sensor is reduced by more than 50 to 80%, and the sensitivity of the sensitive ammeter can reach 10 -7 -10 -12 s, and the response is rapid. Since the FeCo / C working electrode has efficient catalytic activity, the electron transfer rate at both ends of the electrode can be improved. Therefore, using the FeCo / C catalytic material of the present invention as the working electrode can improve the detection sensitivity of electrochemical analysis by more than 40%. Based on the relationship between the measured electric quantity and the degradation performance, it is shown that the sensor of the present invention has the characteristics of detection accuracy, and the matching degree between the linear fitting curve and the test data at each time point exceeds 99.9%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the structure of the electrochemical sensor based on FeCo / C working electrode;
[0024] Figure 2 The degradation curves of tetracycline, chlortetracycline and BPA by FeCo / C working electrode;
[0025] Figure 3 is a current density curve of the electrochemical sensor;
[0026] Figure 4 It is the output charge diagram of the electrochemical sensor;
[0027] Figure 5 is the fitted catalytic curve diagram of the electrochemical sensor;
[0028] Figure 6 It is a comparison chart of the actual degradation curve and the simulated degradation curve. DETAILED DESCRIPTION
[0029] Example 1
[0030] The preparation method of the FeCo / C catalytic material of the present invention specifically comprises the following steps:
[0031] (1) 0.35 g HMIM was dissolved in 2 mL DMF to obtain solution A; 0.8 g Co(NO 3 ) 2 and 0.2gFe(NO 3 ) 3 Dissolve in 1 mL DMF to obtain solution B; stir solution A and solution B separately and fully dissolve;
[0032] (2) Solution B was added to Solution A, and the mixture was reacted for 10 min. After the reaction was complete, 0.2 g PAN was added thereto, and the mixture was stirred at 600 rpm for 20 min to fully dissolve PAN, thereby obtaining a mixed solution.
[0033] (3) 0.7 g of fibrous material was soaked in the above mixed solution and dried in an oven at 80 °C for 60 h;
[0034] (4) Place the dried material in N 2 The catalyst was calcined at 700°C in an atmosphere for 6 to 14 hours, cooled to room temperature and then allowed to stand for 2 hours. The obtained material was taken out and ground into fine powder to obtain a FeCo / C catalytic material.
[0035] The preparation method of the FeCo / C catalytic material in Comparative Example 1 is basically the same as that in Example 1, except that HMIM is not added.
[0036] The preparation method of the FeCo / C catalytic material in Comparative Example 2 is exactly the same as that in Example 1, with the only difference being that the dosage of PAN is 0.05 g.
[0037] The preparation method of the FeCo / C catalytic material in Comparative Example 3 is exactly the same as that in Example 1, with the only difference being that the dosage of PAN is 0.3 g.
[0038] Based on the catalytic materials of Example 1 and Comparative Examples 1 to 3, FeCo / C working electrode I, FeCo / C working electrode II, FeCo / C working electrode III and FeCo / C working electrode IV were prepared respectively by the same method, including the following steps:
[0039] (1) Disperse 90 mg of the catalyst material in 1 mL of NMP, add 10 mg of PVDF, and stir for 1 h to fully dissolve and disperse it evenly;
[0040] (2) Take a 3mm thick, uniform-sized graphite plate and cut it into 3×2cm 2The graphite plate is used as the electrode plate; 100 μL of turbid liquid is dropped on the electrode, and the turbid liquid covers an area of 2×1 cm 2 After the surface layer on one side is dry, turn the electrode over and continue coating; after coating, place it in an oven and dry it at 60°C for 8 hours to obtain FeCo / C working electrode I, FeCo / C working electrode II and FeCo / C working electrode III based on the catalytic materials of Example 1 and Comparative Examples 1 to 3.
[0041] Working electrode I, working electrode II, working electrode III and working electrode IV were respectively used to construct electrochemical sensors for application: the prepared FeCo / C working electrode and graphite electrode were immersed in four identical pollutant solutions, respectively, and the two electrodes were connected in series with the electrical quantity analyzer through a wire to obtain an electrochemical sensor.
[0042] Comparison of the degradation effects of the four working electrodes prepared in Comparative Examples 1 to 3 and Example 1 on BPA: The experimental conditions are BPA concentration of 10 ppm, PMS concentration of 0.5 g / L, electrolyte Na 2 SO 4 The concentration is 0.1 mol / L, and the negative and positive electrode areas are 3×2 cm 2 The concentration of FeCo / C catalyst material loaded on the negative electrode is 10 mg / cm 2 , covering an area of 2×1cm 2 .
[0043] Under the same conditions, the catalytic efficiency of the FeCo / C catalytic material prepared in Example 1 was the best. Within 10 minutes, the BPA degradation rate reached 98.02%, and the sensitivity of the sensitive current meter detection reached 10 -12 The catalytic efficiency of the FeCo / C catalytic material prepared in Comparative Example 1 was the worst, and only 43% of BPA was degraded within 10 min. The sensitivity of the sensitive current meter detection was 10 -7 s, the FeCo / C catalytic material prepared in Comparative Example 2 degraded BPA by 84% within 10 min, and the sensitivity of the sensitive current meter detection reached 10 - 10 The FeCo / C catalytic material prepared in Comparative Example 3 degraded BPA by only 56% within 10 min, and the sensitivity of the sensitive current meter detection reached 10 -8s. HMIM is the organic framework of MOFs. Without HMIM, it is difficult to form ZIFs with high specific surface area, which reduces the specific surface area of the catalyst, resulting in a decrease in active sites, and the ideal catalytic performance and high sensitivity cannot be achieved. As a binder and carbon precursor, the dosage of PAN will affect the catalytic performance and detection sensitivity of FeCo / C catalytic materials. Too little PAN dosage will result in insufficient carbon to coat the FeCo-ZIFs precursor, resulting in a decrease in catalytic stability and detection sensitivity, and will cause the leaching of catalyst metal ions. PAN also acts as a nitrogen source to dope the carbon skeleton with nitrogen, which will further increase the electron transfer rate at both ends of the electrode after nitrogen doping. Too much PAN dosage will also reduce the activity of the catalyst and the sensitivity of the detection. This may be because too much PAN will make it difficult to expose the pore structure of the FeCo / C catalytic material and the catalytic active sites are insufficient.
[0044] like Figure 2 As shown, tetracycline and chlortetracycline were selected as target organic pollutants, and the performance of PMS activation based on the working electrode of the FeCo / C catalytic material in Example 1 for degrading different pollutants was verified: at the same time and the same initial concentration, the FeCo / C catalytic material can achieve efficient removal of organic pollutants. At 10 min, the removal efficiency of tetracycline was 99.67% and the removal efficiency of chlortetracycline was 98.88%, indicating that the FeCo / C catalytic material in Example 1 has excellent catalytic performance.
[0045] Verification of the effectiveness of the sensor of the present invention: The FeCo / C sensor was tested under the same test conditions as the degradation conditions. The current density curve obtained by the test was as follows: Figure 3 As shown by Figure 3 It can be seen that the current density measured by the FeCo / C sensor first increases rapidly and then gradually decreases as the reaction proceeds. This shows that after PMS is added to the system, FeCo / C immediately reacts with PMS to produce a large amount of electron transfer. As the reaction proceeds, the transferred electrons gradually decrease and the current density decreases. This is also verified by the degradation performance. The real-time charge during the degradation process (Q = ∫I t dt), such as Figure 4 According to Faraday's law (Q = zFξ, F is Faraday's constant), there is a certain relationship between the amount of electricity generated during the redox reaction and the progress of the chemical reaction. The natural logarithm of the ratio of the initial concentration of the BPA solution to the BPA concentration at each selected time point has an excellent linear relationship with the output electricity (R 2 =0.9987), the function obtained by fitting can simulate the concentration change of BPA at each time point, such as Figure 5 Comparing the result with the BPA concentration measured by UV-visible spectrophotometer, it is shown that the curve obtained by this method basically coincides with the actual degradation curve, as shown in Figure 2. Figure 6 This curve further confirms the effectiveness of the sensor of the present invention.
Claims
1. A FeCo / C catalytic material, characterized in that: The method is prepared by the following method, which specifically comprises the following steps: (1) Dissolve 2-methylimidazole in N,N-dimethylformamide to obtain solution A; dissolve divalent cobalt salt and trivalent iron salt in N,N-dimethylformamide to obtain solution B; (2) Solution B is added to solution A, and FeCo-ZIFs are rapidly formed in the reaction solution. After the reaction is complete, polyacrylonitrile is added thereto and stirred to dissolve to form a mixed solution of FeCo-ZIFs and polyacrylonitrile. The mixing volume ratio of solution A to solution B is 1.5-2:
1. The reaction time for forming FeCo-ZIFs is 15-25 min. The mass volume ratio of PAN to the reaction solution is 0.06-0.1 g:1 mL, and the dissolution time is 20-30 min. (3) applying the obtained mixed solution on the fibrous material and drying it in an oven, and the FeCo-ZIFs are fixed on the fibrous material through the polyacrylonitrile film; (4) calcining the dried material at high temperature in an inert atmosphere, annealing it, and grinding it to obtain a FeCo / C catalytic material; The BPA concentration is 10ppm, the PMS concentration is 0.5g / L, the electrolyte Na2SO4 concentration is 0.1mol / L, and the negative electrode area is 3×2cm 2 The concentration of FeCo / C catalyst material loaded on the negative electrode is 10 mg / cm 2 , covering an area of 2×1cm 2 ; Within 10 minutes, the BPA degradation rate reached 98.02%.
2. The FeCo / C catalytic material according to claim 1, characterized in that: In step (1), in solution A, the mass concentration of 2-methylimidazole is 0.175~0.180g / mL; in solution B, the mass concentration of the metal salt is 1~1.1g / mL; the divalent cobalt salt is Co(NO3)2; the trivalent iron salt is Fe(NO3)3; and the mass ratio of Co(NO3)2 to Fe(NO3)3 is 4~5:
1.
3. The FeCo / C catalytic material according to claim 1, characterized in that: In step (3), the fibrous material is fiber paper or nylon; the drying temperature is 50-80°C, and the drying time is 60-72 hours.
4. The FeCo / C catalytic material according to claim 1, characterized in that: In step (4), the calcination temperature is 700-1000°C, the calcination time is 6-14 hours, and after cooling to room temperature, the mixture is allowed to stand for 2-5 hours before being taken out.
5. A FeCo / C working electrode based on the FeCo / C catalytic material according to claim 1, characterized in that: The method is prepared by the following method, which specifically comprises the following steps: (1) dispersing FeCo / C catalytic material in N-methylpyrrolidone, adding polyvinylidene fluoride thereto, and obtaining FeCo / C turbid solution; (2) Apply FeCo / C turbid liquid to the filling part on one side of the graphite electrode plate, apply it evenly and then dry it; after it is fully dried, turn the graphite electrode plate over and apply it to the filling part on the other side of the graphite electrode plate, apply it and then dry it to obtain a FeCo / C working electrode.
6. The FeCo / C working electrode according to claim 5, characterized in that: In step (1), the mass volume ratio of the FeCo / C catalytic material to N-methylpyrrolidone is 0.09-0.1 g:1 mL; the mass ratio of the FeCo / C catalytic material to polyvinylidene fluoride is 9-10:
1.
7. The FeCo / C working electrode according to claim 5, characterized in that: In step (2), the area of the coated portion of the graphite electrode plate accounts for 10-80% of the area of the entire electrode plate. The turbid liquid is dripped onto the coated portion of the electrode plate and drained with a rubber-tipped dropper to make it evenly dispersed in the coated portion. The mass area ratio of the FeCo / C catalytic material to the coated portion is 10-15 mg: 1 cm 2 .
8. The FeCo / C working electrode according to claim 5, characterized in that: In step (2), the drying temperature is 50-80°C and the drying time is 8-12 hours.
9. An electrochemical sensor based on the FeCo / C working electrode according to claim 5, characterized in that: It consists of a FeCo / C working electrode, a graphite electrode and a coulometric analyzer, and the two electrodes are connected in series with the coulometric analyzer through a wire.
Citation Information
Patent Citations
Method for treating 6-nitrate wastewater by aid of electrolysis joint processes
CN106830454A
Method for preparing hollow carbon fiber material for supercapacitor
CN106835363A
Preparation method and application of iron doped cobalt diselenide compound nitrogen doped carbon material
CN108374179A
Method for nitrogen-doped graphene aerogel electrode electro-catalysis degraded cephalosporin
CN108751352A
Ti3C2-FeCo composite transition metal catalyst, and preparation method and application thereof
CN109012717A