A polysilicon high boiling point impurity remover and its application
By using impurities removal agents composed of composite alkali metal chloride and amino carboxylate, a bonding system is formed through distillation treatment, and the aluminum and titanium impurities in the high boiling substance of polycrystalline silicon are efficiently removed, solving the problem of removal in the prior art and realizing the realization of Efficient and low-cost metal impurity separation.
Patent Information
- Application Number
- CN202310074196.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-02-07
AI Technical Summary
The prior art is difficult to efficiently remove metal impurities such as aluminum and titanium in high boiling substances of polycrystalline silicon, resulting in high catalyst losses, increased production costs and unstable treatment processes.
A polycrystalline silicon high-boiler impurity removal agent composed of alkali metal chloride and amino carboxylate salt is used to form a bonding system for aluminum and titanium impurities and impurity removal agents through distillation, which significantly improves the separation efficiency.
The removal rates of aluminum and titanium in high boiling substances of polycrystalline silicon are achieved by more than 95%, reducing catalyst consumption, improving production cost-effectiveness, and simplifying the processing flow.
Abstract
Description
Technical Field
[0001] The invention relates to a polysilicon high boiling point impurity remover and application thereof, belonging to the field of chemistry. Background Art
[0002] Polysilicon is the basic raw material of the photovoltaic industry, and some by-products are produced during its preparation process. Some of these by-products are high-boiling compounds (commonly known as "high-boiling substances") with a boiling point exceeding 70°C, and their mass accounts for 7.0% to 8.0% of the crude monomer product. 99% of these high-boiling substances are polychlorosilanes, which have very complex components and the boiling points of each component are relatively close. It is difficult to separate the components by commonly used separation methods, so they cannot be effectively utilized. In the actual production process, the main treatment method for high-boiling substances is to concentrate and separate them, recover a part of the low-boiling substances such as silicon tetrachloride remaining in the high-boiling substances, and then hydrolyze the remaining high-boiling substances together with solid impurities brought out during the processing of other polysilicon such as metal chlorides. Although this treatment method is simple and effective, it consumes a large amount of Si and Cl elements that should be valuable, which is not conducive to the sustainable development of polysilicon production. In addition, if these high-boiling substances are not handled properly, it will increase the production costs of enterprises and cause safety and environmental problems.
[0003] In order to solve the above problems, people have developed a method of using organic amines as catalysts to catalyze the cracking of polychlorosilane into monosilicon compounds, that is, using tributylamine, tri-n-octylamine, N,N-diethylaniline, N,N-diethylbutylamine, etc. as catalysts to crack high-boiling products into monosilicon compounds for recycling. However, high-boiling products contain some metal impurities, among which aluminum trichloride and titanium tetrachloride impurities are the most representative, and the mass content of these two metal elements can reach hundreds to thousands of ppm. The metal impurities in high-boiling products will react with the organic amines in the catalyst, causing a large loss of cracking catalysts during the catalytic cracking process. In order to ensure the catalytic effect, it is necessary to continuously replenish the lost catalyst during the cracking process, which not only increases the operating cost, but also seriously affects the stability of the production process. Under normal pressure conditions, the boiling point of titanium tetrachloride is 135-136°C, and the boiling point of aluminum trichloride is 182.7°C, but sublimation will occur at 177.8°C. These temperatures are very close to the distillation range of high boiling products (120-180°C), so it is difficult to separate the two metal chlorides from other components in the high boiling products by conventional distillation treatment and the like.
[0004] The current prior art can provide some methods to avoid the loss of catalysts caused by metal impurities. For example, patent CN108658082A discloses a method for removing aluminum chloride by pre-treating high-boiling substances. The method is to send the high-boiling substances to a cooling and stirring tank, stir them at low temperature for 1-5 hours, send them to a sedimentation tank, and then let the high-boiling substances settle in a nitrogen environment for 1-20 hours, thereby separating the slurry including solid impurities and metal halides. However, this method has a long processing flow and the effect of removing aluminum chloride is not ideal; patent CN113149017A discloses a complexing agent for removing aluminum from polysilicon high-boiling substances and its application, and the structure of the complexing agent is complex. The invention discloses a method for removing aluminum chloride from high-boiling substances, wherein an auxiliary agent and aluminum-containing impurities are first added to the high-boiling substances to form a mixed system containing non-volatile aluminum compounds, and then the remaining components in the high-boiling substances are separated from the mixed system by distillation, thereby removing aluminum chloride impurities. However, the auxiliary agent used in the method is prepared by mixing "deferoxamine", "deferiprone" and "testiron" in a certain proportion, and the iron removal effect is relatively high, but the aluminum removal effect is not ideal, and the cost is also relatively high.
[0005] Therefore, developing a low-cost and highly efficient treatment agent for removing metal impurities such as aluminum and titanium from high-boiling products of polysilicon is an urgent problem to be solved in the art. Summary of the invention
[0006] The invention provides a polysilicon high boiling point impurity remover, which has a simple composition and cheap and readily available raw materials. After the impurity remover is added to the polysilicon high boiling point, the polysilicon high boiling point and metal impurities can be efficiently separated by distillation.
[0007] The present invention also provides a method for removing metal impurities from high boiling polysilicon products. The method can effectively separate the metal impurities from the high boiling polysilicon products by selecting a suitable impurity remover, mixing the mixture with the high boiling polysilicon products and performing a distillation treatment.
[0008] The invention provides a polysilicon high-boiling-point impurity remover, which comprises, in parts by mass: 90 to 100 parts of a compounded alkali metal chloride and 80 to 90 parts of an aminocarboxylate.
[0009] The polysilicon high boiling point impurity remover as described above, wherein the composite alkali metal chloride includes at least two of lithium chloride, sodium chloride and potassium chloride.
[0010] In the polysilicon high boiling point impurity remover as described above, the compound alkali metal chloride may be a combination of sodium chloride and potassium chloride.
[0011] In the polysilicon high boiling point impurity remover as described above, the mass ratio of sodium chloride to potassium chloride is 100:1 to 100:20.
[0012] The polysilicon high boiling point impurity remover as described above, wherein the aminocarboxylate is selected from at least one of trisodium nitrilotriacetate, potassium nitrilotriacetate, disodium ethylenediaminetetraacetate, dipotassium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, tetrapotassium ethylenediaminetetraacetate, sodium 1,3-propylenediaminetetraacetate, and potassium 1,3-propylenediaminetetraacetate.
[0013] The present invention also provides a method for removing metal impurities from high-boiling polysilicon products, wherein the high-boiling polysilicon product remover described in any of the above items is mixed with the high-boiling polysilicon product to obtain a mixed system, and the mixed system is distilled to obtain the high-boiling polysilicon product after impurities are removed.
[0014] In the method for removing metal impurities from high boiling points of polysilicon as described above, the mass ratio of the polysilicon high boiling point remover to the polysilicon high boiling point is 1:(20-80).
[0015] In the method for removing metal impurities from high boiling points of polysilicon as described above, the temperature of the distillation treatment is 140°C to 180°C.
[0016] In the method for removing metal impurities from high boiling points of polysilicon as described above, during the distillation process, the heating rate of the mixed system is 5° C. / min.
[0017] In the method for removing metal impurities from high boiling points of polysilicon as described above, the pressure of the distillation treatment is 0.1 MPa to 1.0 MPa.
[0018] The present invention provides a polysilicon high boiling point impurity remover, which can remove aluminum and titanium metal impurities in the polysilicon high boiling point by selecting appropriate raw materials and matching them in a certain ratio, and then mixing them with the polysilicon high boiling point, and then treating them by distillation, so that the removal rate of aluminum and titanium metal impurities in the polysilicon high boiling point can reach more than 95% (by mass fraction). The use of the polysilicon high boiling point impurity remover helps to reduce the loss of the organic amine catalyst caused by metal impurities in the process of using organic amine to catalyze the cracking of polychlorosilane in the high boiling point into monosilane, thereby reducing the production cost of the polysilicon high boiling point cracking process. DETAILED DESCRIPTION
[0019] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0020] The first aspect of the present invention provides a polysilicon high-boiling-point impurity remover, which comprises, in parts by mass: 90 to 100 parts of a compounded alkali metal chloride and 80 to 90 parts of an aminocarboxylate.
[0021] The compound alkali metal chloride referred to in the present invention is a mixture of at least two alkali metal salts, wherein the cation of the alkali metal salt is a Group IA metal ion and the anion is a chloride ion. The aminocarboxylate referred to in the present invention is a carboxylate compound of a tertiary amine, and each hydrocarbon group in the tertiary amine is substituted by at least one carboxyl group. It should be noted that, in addition to the carboxyl group, the present invention does not limit other forms of hydrocarbon groups.
[0022] At present, when the high-boiling polysilicon product is directly subjected to distillation treatment, the aluminum and titanium impurities in the high-boiling product will be distilled out as a fraction along with the high-boiling product. When the above-mentioned impurity remover of the present invention is added to the high-boiling polysilicon product, under the same conditions, the content of aluminum and titanium impurities in the high-boiling product fraction distilled out will be significantly reduced. Based on this phenomenon, the inventor analyzed the impurity removal principle and speculated that the reason may be: the impurity remover of the present invention can bond with aluminum impurities and titanium impurities under heating conditions to form a bonding system, and the boiling point of the bonding system is significantly higher than that of the high-boiling polysilicon product. Therefore, when the distillation treatment is carried out, most of the aluminum impurities and titanium impurities can be left in the distillation system in the form of new substances, thereby obtaining the high-boiling polysilicon product after the removal of aluminum and titanium.
[0023] Therefore, by using the treatment agent of the present invention as a de-impurity agent for high-boiling products of polysilicon, the aluminum and titanium contents in the high-boiling products of polysilicon can be significantly reduced, thereby reducing the consumption of organic amine catalysts during the catalytic cracking of high-boiling products of polysilicon, thereby improving the utilization rate of high-boiling products of polysilicon at a lower production cost.
[0024] The alkali metal chloride and aminocarboxylate in the polysilicon high boiling point impurity remover of the present invention can be selected from cheap and readily available raw materials in the art, and therefore, compared with the complex structure treating agents used in the prior art, it also has the advantages of low cost and high economic benefit.
[0025] The present invention does not limit the preparation method of the impurity remover, as long as the compound alkali metal chloride and the aminocarboxylate are mixed in the above ratio. In a specific embodiment, when the mixed system after the above compound alkali metal chloride and the aminocarboxylate are mixed in proportion is subjected to ball milling treatment and sieving treatment (120 mesh) in sequence, the impurity remover for polysilicon high boiling point is better. The reason may be that the above ball milling treatment and sieving treatment help to improve the dispersibility of the impurity remover in the polysilicon high boiling point, so that the impurity remover and the polysilicon high boiling point have sufficient contact area, thereby improving the impurity removal effect.
[0026] In a specific implementation process, illustratively, the mixed system is ball-milled in a ball mill for 1 hour and then placed in a vibrating screen and passed through a 120-mesh stainless steel screen to obtain the impurity remover of the present invention.
[0027] The composite alkali metal chloride of the present invention is selected from two or more of lithium chloride, sodium chloride and potassium chloride, and is more preferably a combination of sodium chloride and potassium chloride.
[0028] In the specific implementation process, the inventors found that compared with using LiCl and KCl or LiCl and NaCl to form a composite alkali metal chloride, when NaCl and KCl are used to form a composite alkali metal chloride, the polysilicon high-boiling-point impurity remover containing this composite alkali metal chloride is more effective in removing metal impurities.
[0029] Furthermore, when the mass ratio of sodium chloride to potassium chloride is 100:1 to 100:20, the effect of removing metal impurities is more prominent. Furthermore, when the mass ratio is 100:2.5 to 100:10, the effect of removing metal impurities is more prominent.
[0030] The aminocarboxylate of the present invention is selected from at least one of trisodium nitrilotriacetate, potassium nitrilotriacetate, disodium ethylenediaminetetraacetate, dipotassium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, tetrapotassium ethylenediaminetetraacetate, sodium 1,3-propylenediaminetetraacetate, and potassium 1,3-propylenediaminetetraacetate, and more preferably at least one of disodium ethylenediaminetetraacetate, dipotassium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, and tetrapotassium ethylenediaminetetraacetate.
[0031] The second aspect of the present invention provides a method for removing metal impurities from polysilicon high boiling points. Specifically, the polysilicon high boiling point remover of the first aspect is mixed with the polysilicon high boiling point to obtain a mixed system, and the mixed system is distilled to obtain the polysilicon high boiling point after impurities are removed.
[0032] In the above method, the process of heating the polysilicon high boiling point impurity remover after mixing with the polysilicon high boiling point and then performing distillation treatment is a process in which the impurity remover interacts with the aluminum and titanium impurities in the polysilicon high boiling point to form a new substance; utilizing the difference between the boiling point of the new substance and the distillation range of the polysilicon high boiling point, the aluminum and titanium impurities remain in the distillation container through distillation treatment, and the polysilicon high boiling point is distilled out as a fraction. The fraction produced in the distillation treatment is condensed and collected, and the fraction is the polysilicon high boiling point from which the aluminum and titanium impurities have been removed.
[0033] Furthermore, when the mass ratio of the polysilicon high boiling point impurity remover to the polysilicon high boiling point is controlled to be 1:(20-80), preferably 1:(20-60), a better impurity removal effect can be obtained.
[0034] According to the difference in boiling point between the impurity system after treatment and the high boiling point of polysilicon, the temperature of the distillation treatment can be controlled to be 140°C to 180°C, preferably 152°C to 177°C.
[0035] In order to make the polysilicon high-boiling impurity remover work better, it is necessary to control the heating rate of the mixed system composed of high boiling substances and impurity removers during distillation treatment. The inventors found that when the heating rate of the distillation treatment is 5°C / min, the impurity removal effect of aluminum and titanium impurities is better than the experimental results obtained at other heating rates. The inventors speculate that the reason may be that at this heating rate, the polysilicon high-boiling impurity remover can better combine with metal impurities, thereby better exerting the impurity removal effect.
[0036] The present invention has no particular limitation on the pressure of the distillation treatment, and there is no need to use harsh high pressure or negative pressure conditions. In a specific embodiment, the pressure of the distillation treatment is 0.1 MPa to 1.0 MPa, preferably controlled to be 0.1 MPa to 0.4 MPa.
[0037] The following will further describe in detail the treatment agent for removing aluminum from high boiling points of polysilicon and its application provided by the present invention in conjunction with specific embodiments.
[0038] In the following examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.
[0039] In the following examples, the Al content of the high-boiling products of polysilicon to be treated and the condensed and collected distillates after treatment are determined according to the method given in Section 5.5. "Determination of iron, aluminum, chromium, titanium, copper, manganese, nickel, boron and phosphorus contents" of China Chemical Industry Standard HG / T 5745-2020, and the unit wppm refers to one part per million by mass.
[0040] Example 1
[0041] The polysilicon high boiling point impurity remover of this embodiment is composed of the following raw materials in terms of mass fractions: 89.1 parts of NaCl, 13.4 parts of KCl and 91.6 parts of disodium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and the polysilicon high boiling point impurity remover of this embodiment is prepared after being sieved through a 120-mesh stainless steel screen.
[0042] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0043] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (Al content is 930 wppm, Ti content is 2945 wppm) are added into a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0044] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain the temperature thereafter. The operating pressure is controlled at 0.1 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0045] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0046] The Al content of the condensed and collected evaporation was measured to be 18wppm and the Ti content was 35wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 98.1%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 98.8%.
[0047] Example 2
[0048] The polysilicon high boiling point impurity remover of this embodiment is composed of the following raw materials in terms of mass fractions: 95.8 parts of NaCl, 6.7 parts of KCl and 91.6 parts of disodium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and sieved through a 120-mesh stainless steel screen to prepare the polysilicon high boiling point impurity remover of this embodiment.
[0049] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0050] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (with an Al content of 865 wppm and a Ti content of 2684 wppm) were added to a reactor, the top outlet of the reactor was connected to a condenser via a back pressure valve, and stirring was turned on to fully mix the polysilicon high boiling point impurity remover with the polysilicon high boiling point;
[0051] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain the temperature thereafter. The operating pressure is controlled at 0.1 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0052] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0053] The Al content of the condensed and collected evaporation was measured to be 14wppm and the Ti content was 27wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 98.4%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 99.0%.
[0054] Example 3
[0055] The polysilicon high boiling point impurity remover of the present embodiment is composed of the following raw materials in terms of mass fractions: 95.8 parts of NaCl, 6.7 parts of KCl, 54.9 parts of disodium ethylenediaminetetraacetate and 36.7 parts of tetrasodium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and the polysilicon high boiling point impurity remover of the present embodiment is prepared after being sieved through a 120-mesh stainless steel screen.
[0056] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0057] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (with an Al content of 860 wppm and a Ti content of 2690 wppm) are added to a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, and stirring is turned on to fully mix the polysilicon high boiling point impurity remover and the polysilicon high boiling point;
[0058] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0059] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0060] The Al content of the condensed and collected evaporation was measured to be 15wppm and the Ti content was 22wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 98.3%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 99.2%.
[0061] Example 4
[0062] The polysilicon high boiling point impurity remover of the present embodiment is composed of the following raw materials in terms of mass fractions: 95.8 parts of NaCl, 6.7 parts of KCl, 54.9 parts of dipotassium ethylenediaminetetraacetate and 36.7 parts of tetrapotassium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and sieved through a 120-mesh stainless steel screen to prepare the polysilicon high boiling point impurity remover of the present embodiment.
[0063] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0064] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (Al content is 924 wppm, Ti content is 3050 wppm) are added to a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0065] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0066] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0067] The Al content of the condensed and collected evaporation was measured to be 15wppm and the Ti content was 22wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 98.4%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 99.3%.
[0068] Example 5
[0069] The polysilicon high boiling point impurity remover of this embodiment is composed of the following raw materials in terms of mass fractions: 95.8 parts of NaCl, 6.7 parts of KCl, 54.9 parts of 1,3-propylenediaminetetraacetic acid sodium and 36.7 parts of 1,3-propylenediaminetetraacetic acid potassium. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and the polysilicon high boiling point impurity remover of this embodiment is prepared after being sieved through a 120-mesh stainless steel screen.
[0070] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0071] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (with an Al content of 886 wppm and a Ti content of 3120 wppm) were added to a reactor, the top outlet of the reactor was connected to a condenser via a back pressure valve, and stirring was turned on to fully mix the polysilicon high boiling point impurity remover and the polysilicon high boiling point;
[0072] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0073] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0074] The Al content of the condensed and collected evaporation was measured to be 17wppm and the Ti content was 131wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 98.1%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 95.8%.
[0075] Example 6
[0076] The polysilicon high boiling point impurity remover of the present embodiment is composed of the following raw materials in terms of mass fractions: 95.8 parts of NaCl, 6.7 parts of KCl, 54.9 parts of disodium ethylenediaminetetraacetate and 36.7 parts of dipotassium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and the polysilicon high boiling point impurity remover of the present embodiment is prepared after being sieved through a 120-mesh stainless steel screen.
[0077] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0078] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (Al content is 942 wppm, Ti content is 2781 wppm) are added to the reactor, the top outlet of the reactor is connected to the condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0079] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0080] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0081] The Al content of the condensed and collected evaporation was measured to be 14wppm and the Ti content was 36wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 98.5%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 98.7%.
[0082] Example 7
[0083] The polysilicon high boiling point impurity remover of the present embodiment is composed of the following raw materials in terms of mass fractions: 95.8 parts of NaCl, 6.7 parts of KCl, 54.9 parts of disodium ethylenediaminetetraacetate, 25.7 parts of tetrasodium ethylenediaminetetraacetate and 11 parts of dipotassium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and the polysilicon high boiling point impurity remover of the present embodiment is prepared after being sieved through a 120-mesh stainless steel screen.
[0084] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0085] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (Al content is 946 wppm, Ti content is 2921 wppm) are added to a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0086] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0087] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0088] The Al content of the condensed and collected evaporation was measured to be 15wppm and the Ti content was 20wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 98.4%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 99.3%.
[0089] Example 8
[0090] The polysilicon high boiling point impurity remover of the present embodiment is composed of the following raw materials in terms of mass fractions: 99.2 parts of NaCl, 3.3 parts of KCl, 54.9 parts of disodium ethylenediaminetetraacetate, 25.7 parts of tetrasodium ethylenediaminetetraacetate and 11 parts of dipotassium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and the polysilicon high boiling point impurity remover of the present embodiment is prepared after being sieved through a 120-mesh stainless steel screen.
[0091] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0092] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (with an Al content of 883 wppm and a Ti content of 3024 wppm) were added to a reactor, the top outlet of the reactor was connected to a condenser via a back pressure valve, and stirring was turned on to fully mix the polysilicon high boiling point impurity remover and the polysilicon high boiling point;
[0093] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0094] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0095] The Al content of the condensed and collected evaporation was measured to be 7wppm and the Ti content was 30wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 99.2%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 99.0%.
[0096] Example 9
[0097] The polysilicon high boiling point impurity remover of the present embodiment is composed of the following raw materials in terms of mass fractions: 99.2 parts of NaCl, 3.3 parts of KCl, 82.4 parts of disodium ethylenediaminetetraacetate, 12.8 parts of tetrasodium ethylenediaminetetraacetate and 5.5 parts of dipotassium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and the polysilicon high boiling point impurity remover of the present embodiment is prepared after being sieved through a 120-mesh stainless steel screen.
[0098] The method for removing metal impurities in polysilicon high boiling points in this embodiment comprises the following steps:
[0099] 1) 1 g of the polysilicon high boiling point impurity remover of this embodiment and 50 g of the polysilicon high boiling point to be treated (Al content is 878 wppm, Ti content is 3006 wppm) are added to a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0100] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0101] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0102] The Al content of the condensed and collected evaporation was measured to be 6wppm and the Ti content was 15wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this embodiment is 99.3%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 99.5%.
[0103] Example 10
[0104] This embodiment is basically the same as the embodiment 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of LiCl, 13.4 parts of KCl and 91.6 parts of disodium ethylenediaminetetraacetate.
[0105] According to the calculation method of Example 1, the aluminum removal rate of this example is 78.4%, and the titanium removal rate is 96.3%.
[0106] Embodiment 11
[0107] This embodiment is basically the same as the embodiment 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 13.4 parts of LiCl and 91.6 parts of disodium ethylenediaminetetraacetate.
[0108] According to the calculation method of Example 1, the aluminum removal rate of this example is 87.9%, and the titanium removal rate is 97.1%.
[0109] Example 12
[0110] This embodiment is basically the same as the embodiment 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 8.9 parts of KCl and 91.6 parts of disodium ethylenediaminetetraacetate.
[0111] According to the calculation method of Example 1, the aluminum removal rate of this example is 97.2%, and the titanium removal rate is 98.5%.
[0112] Embodiment 13
[0113] This embodiment is basically the same as the embodiment 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 4.5 parts of KCl and 91.6 parts of disodium ethylenediaminetetraacetate.
[0114] According to the calculation method of Example 1, the aluminum removal rate of this example is 98.7%, and the titanium removal rate is 99.1%.
[0115] Embodiment 14
[0116] This embodiment is basically the same as the embodiment 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 2.2 parts of KCl and 91.6 parts of disodium ethylenediaminetetraacetate.
[0117] According to the calculation method of Example 1, the aluminum removal rate of this example is 98.6%, and the titanium removal rate is 97.9%.
[0118] Embodiment 15
[0119] This embodiment is basically the same as the embodiment 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 1.5 parts of KCl and 91.6 parts of disodium ethylenediaminetetraacetate.
[0120] According to the calculation method of Example 1, the aluminum removal rate of this example is 96.6%, and the titanium removal rate is 96.7%.
[0121] Example 16
[0122] This embodiment is basically the same as the embodiment 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 1.1 parts of KCl and 91.6 parts of disodium ethylenediaminetetraacetate.
[0123] According to the calculation method of Example 1, the aluminum removal rate of this example is 96.2%, and the titanium removal rate is 96.1%.
[0124] Embodiment 17
[0125] This embodiment is basically the same as the embodiment 1, except that 5 g of the polysilicon high boiling point remover of this embodiment and 50 g of the polysilicon high boiling point to be treated in the embodiment 1 are added into the reactor.
[0126] According to the calculation method of Example 1, the aluminum removal rate of this example is 96.9%, and the titanium removal rate is 97.1%.
[0127] Embodiment 18
[0128] This embodiment is basically the same as the embodiment 1, except that 2.5 g of the polysilicon high boiling point remover of this embodiment and 50 g of the polysilicon high boiling point to be treated in the embodiment 1 are added into the reactor.
[0129] According to the calculation method of Example 1, the aluminum removal rate of this example is 97.5%, and the titanium removal rate is 97.8%.
[0130] Embodiment 19
[0131] This embodiment is basically the same as the embodiment 1, except that 1.3 g of the polysilicon high boiling point remover of this embodiment and 50 g of the polysilicon high boiling point to be treated in the embodiment 1 are added into the reactor.
[0132] According to the calculation method of Example 1, the aluminum removal rate of this example is 97.9%, and the titanium removal rate is 98.5%.
[0133] Embodiment 20
[0134] This embodiment is basically the same as the embodiment 1, except that 0.8 g of the polysilicon high boiling point remover of this embodiment and 50 g of the polysilicon high boiling point to be treated in the embodiment 1 are added into the reactor.
[0135] According to the calculation method of Example 1, the aluminum removal rate of this example is 97.8%, and the titanium removal rate is 98.0%.
[0136] Embodiment 21
[0137] This embodiment is basically the same as the embodiment 1, except that 0.6 g of the polysilicon high boiling point remover of this embodiment and 50 g of the polysilicon high boiling point to be treated in the embodiment 1 are added into the reactor.
[0138] According to the calculation method of Example 1, the aluminum removal rate of this example is 97.1%, and the titanium removal rate is 97.3%.
[0139] Comparative Example 1
[0140] The method for removing aluminum chloride impurities in polysilicon high boiling products in this comparative example comprises the following steps:
[0141] 1) 50 g of polysilicon high boiling products to be treated (Al content of 930 wppm, Ti content of 2945 wppm) were added into the reactor, the top outlet of the reactor was connected to the condenser via a back pressure valve, and stirring was started;
[0142] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0143] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0144] The Al content of the condensed and collected evaporation was measured to be 895wppm and the Ti content was 2903wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this comparative example is 3.7%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 1.4%.
[0145] Comparative Example 2
[0146] In this comparative example, 1 g of ZnCl2 was added into a ball mill and ball-milled for 3 hours, and then put into a vibrating screen, and the polysilicon high-boiling-point impurity remover was prepared after being screened out through a 120-mesh stainless steel screen.
[0147] The method for removing metal impurities in polysilicon high boiling products of this comparative example comprises the following steps:
[0148] 1) 1 g of the polysilicon high boiling point impurity remover of this comparative example and 50 g of the polysilicon high boiling point to be treated (Al content is 886 wppm, Ti content is 2696 wppm) are added into a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0149] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0150] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0151] The Al content of the condensed and collected evaporation was measured to be 433wppm, and the Ti content was 2663wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this comparative example is 51.1%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 1.2%.
[0152] Comparative Example 3
[0153] The polysilicon high boiling point impurity remover of this comparative example is composed of the following raw materials in parts by mass: 89.1 parts of NaCl and 13.4 parts of KCl. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and sieved through a 120-mesh stainless steel screen to prepare the polysilicon high boiling point impurity remover of this comparative example.
[0154] The method for removing metal impurities in polysilicon high boiling products of this comparative example comprises the following steps:
[0155] 1) 1 g of the polysilicon high boiling point impurity remover of this comparative example and 50 g of the polysilicon high boiling point to be treated (Al content is 930 wppm, Ti content is 3129 wppm) are added into a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0156] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0157] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0158] The Al content of the condensed and collected evaporation was measured to be 17wppm and the Ti content was 3064wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this comparative example is 98.2%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 2.1%.
[0159] Comparative Example 4
[0160] The polysilicon high boiling point impurity remover of this comparative example is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 13.4 parts of KCl, 45.8 parts of deferoxamine (CAS No. 70-51-9) and 45.8 parts of deferiprone (CAS No. 30621-11-0). The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and the polysilicon high boiling point impurity remover of this comparative example is prepared after being sieved through a 120-mesh stainless steel screen.
[0161] The method for removing metal impurities in polysilicon high boiling products of this comparative example comprises the following steps:
[0162] 1) 1 g of the polysilicon high boiling point impurity remover of this comparative example and 50 g of the polysilicon high boiling point to be treated (Al content is 889 wppm, Ti content is 3159 wppm) are added into a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0163] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0164] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0165] The Al content of the condensed and collected evaporation was measured to be 12wppm, and the Ti content was 982wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this comparative example is 98.7%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 68.9%.
[0166] Comparative Example 5
[0167] The polysilicon high boiling point impurity remover of this comparative example is composed of the following raw materials in parts by mass: 82.4 parts of disodium ethylenediaminetetraacetate, 12.8 parts of tetrasodium ethylenediaminetetraacetate and 5.5 parts of dipotassium ethylenediaminetetraacetate. The above raw materials are added to a ball mill and ball milled for 1 hour, then put into a vibrating screen, and sieved through a 120-mesh stainless steel screen to prepare the polysilicon high boiling point impurity remover of this comparative example.
[0168] The method for removing metal impurities in polysilicon high boiling products of this comparative example comprises the following steps:
[0169] 1) 1 g of the polysilicon high boiling point impurity remover of this comparative example and 50 g of the polysilicon high boiling point to be treated (Al content is 802wppm, Ti content is 3062wppm) are added into a reactor, the top outlet of the reactor is connected to a condenser via a back pressure valve, stirring is turned on, and the polysilicon high boiling point impurity remover and the polysilicon high boiling point are fully mixed;
[0170] 2) Maintain stirring, and raise the temperature of the reactor to 155°C at a heating rate of 5°C / min and maintain it thereafter. The operating pressure is controlled at 0.2 MPa by a back pressure regulating valve. The volatile substances in the reactor are condensed by a condenser and collected in a container connected to the condenser.
[0171] 3) When no more volatile substances continue to condense and be produced, the heating is stopped and the biological residues in the reactor are discharged.
[0172] The Al content of the condensed and collected evaporation was measured to be 284wppm and the Ti content was 116wppm. Through calculation, it can be known that the aluminum removal rate (aluminum removal rate = 1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated × 100%) of this comparative example is 64.6%. The titanium removal rate (titanium removal rate = 1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated × 100%) is 96.2%.
[0173] Comparative Example 6
[0174] This comparative example is basically the same as Example 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 13.4 parts of KCl and 45.8 parts of disodium ethylenediaminetetraacetate.
[0175] According to the calculation method of Example 1, the aluminum removal rate of this comparative example is 90.4%, and the titanium removal rate is 89.7%.
[0176] Comparative Example 7
[0177] This comparative example is basically the same as Example 1, except that the polysilicon high boiling point impurity remover is composed of the following raw materials in parts by mass: 89.1 parts of NaCl, 13.4 parts of KCl and 153.8 parts of disodium ethylenediaminetetraacetate.
[0178] According to the calculation method of Example 1, the aluminum removal rate of this comparative example is 84.6%, and the titanium removal rate is 92.2%.
[0179] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some or all of the technical features can be replaced by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for removing metal impurities from high boiling products of polysilicon, characterized in that: Using a polysilicon high boiling point impurity remover, the polysilicon high boiling point impurity remover comprises, by weight: 90 to 100 parts of a composite alkali metal chloride and 80 to 90 parts of an aminocarboxylate; The composite alkali metal chloride includes at least two of lithium chloride, sodium chloride and potassium chloride; The aminocarboxylate is selected from at least one of trisodium nitrilotriacetate, potassium nitrilotriacetate, disodium ethylenediaminetetraacetate, dipotassium ethylenediaminetetraacetate, tetrasodium ethylenediaminetetraacetate, tetrapotassium ethylenediaminetetraacetate, sodium 1,3-propylenediaminetetraacetate, and potassium 1,3-propylenediaminetetraacetate; The method for removing metal impurities from polysilicon high boiling points comprises: mixing the polysilicon high boiling point remover with the polysilicon high boiling point to obtain a mixed system, and performing distillation treatment on the mixed system to obtain the polysilicon high boiling point after impurities are removed.
2. The method for removing metal impurities in high boiling products of polysilicon according to claim 1, characterized in that: The composite alkali metal chloride is a combination of sodium chloride and potassium chloride.
3. The method for removing metal impurities from high boiling points of polysilicon according to claim 1 or 2, characterized in that: The mass ratio of sodium chloride to potassium chloride is 100:1 to 100:
20.
4. The method for removing metal impurities in high boiling products of polysilicon according to claim 1, characterized in that: The mass ratio of the polysilicon high boiling point impurity remover to the polysilicon high boiling point is 1:(20-80).
5. The method for removing metal impurities from high boiling points of polysilicon according to claim 4, characterized in that: The temperature of the distillation treatment is 140°C to 180°C.
6. The method for removing metal impurities from high boiling points of polysilicon according to claim 4, characterized in that: During the distillation process, the heating rate of the mixed system is 5°C / min.
7. The method for removing metal impurities from high boiling points of polysilicon according to claim 5, characterized in that: During the distillation process, the heating rate of the mixed system is 5°C / min.
8. The method for removing metal impurities from high boiling points of polysilicon according to claim 4, characterized in that: The pressure of the distillation treatment is 0.1 MPa to 1.0 MPa.
9. The method for removing metal impurities from high boiling points of polysilicon according to claim 5, characterized in that: The pressure of the distillation treatment is 0.1 MPa to 1.0 MPa.
10. The method for removing metal impurities from high boiling points of polysilicon according to claim 6, characterized in that: The pressure of the distillation treatment is 0.1 MPa to 1.0 MPa.
11. The method for removing metal impurities from high boiling points of polysilicon according to claim 7, characterized in that: The pressure of the distillation treatment is 0.1 MPa to 1.0 MPa.