A kind of thermal insulation layer plastering gypsum and preparation process thereof
By using antibacterial aerogels of nanotitanium dioxide and nanometal zinc in plaster plaster, the problem of mold breeding in humid areas is solved, and its stable antibacterial and anti-mold and hydrophobic effects are achieved, reducing the risk of steel bar oxidation.
Patent Information
- Application Number
- CN202310223702.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-09
AI Technical Summary
Plastering plaster is prone to absorb water in humid areas and mold breeds, affecting its use.
An antibacterial aerogel containing nanotitanium dioxide and nanometal zinc is used as components. Through its pore structure and the catalytic action of zinc ionic compounds, the antibacterial and hydrophobic properties of plaster gypsum are significantly improved, and the possibility of mold reproduction and reinforcement oxidation is reduced.
It effectively reduces the humidity and mold reproduction risk of plaster plaster, enhances its antibacterial and mildew-proof properties, and reduces the possibility of steel bar corrosion.
Smart Images

Figure BDA0004117780580000091 
Figure BDA0004117780580000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building materials, and more specifically, to a thermal insulation layer plastering gypsum and a preparation process thereof. Background Art
[0002] Plastering gypsum is a mixture of hemihydrate gypsum (CaSO4·1 / 2H2O) and type II anhydrous calcium sulfate (type II CaSO 4) Plastering materials made of cementitious materials, either alone or mixed with other materials, are made of admixtures. Plastering gypsum has the strength of cement, but is healthier, more environmentally friendly, more durable, has strong bonding strength, is not easy to powder, crack, hollow, or fall off, and is easy to use and has a low cost. Therefore, it has become an environmentally friendly decorative material that is promoted by the country.
[0003] However, plastering gypsum is extremely water-resistant. Therefore, when plastering gypsum is used in moist areas for a long time, it is easy for the plastering gypsum to absorb water and cause mold growth, which in turn affects the normal use of the plastering gypsum. Summary of the invention
[0004] In order to improve the problem that mold is easily grown on plaster in humid areas, the present application provides an insulating layer plaster and a preparation process thereof.
[0005] In the first aspect, the present application provides a thermal insulation layer plastering gypsum, which adopts the following technical solution:
[0006] A thermal insulation layer plastering gypsum is composed of the following raw materials in parts by weight: 80-90 parts of gypsum powder, 1-3 parts of alkaline agent, 0.1-0.3 parts of water retaining agent, 0.02-0.10 parts of retarder, 0.02-0.04 parts of thixotropic agent, 0.02-0.04 parts of air entraining agent, 5-10 parts of lightweight filler and 5-10 parts of antibacterial aerogel, wherein the antibacterial aerogel contains nano titanium dioxide and nano metal zinc, and a small amount of zinc ion compound is formed on the surface of the nano metal zinc.
[0007] Since the antibacterial aerogel itself has a rich porous structure, after the house is decorated, the antibacterial aerogel can also adsorb formaldehyde, and formaldehyde can react with the amino group of bacterial protein or the thiol group in the bacterial enzyme system through nucleophilic addition, causing the bacteria to lose their ability to replicate and causing metabolic system disorders, thereby achieving the purpose of sterilization and inhibition. When the amount of formaldehyde adsorbed is too large, the titanium dioxide and zinc ion compounds in the antibacterial aerogel can catalyze the decomposition of formaldehyde.
[0008] Zinc ion compounds also have excellent antibacterial properties. The antibacterial mechanism is that during the use of zinc ion compounds, the zinc ions of the zinc ion compounds are gradually released. When the zinc ions come into contact with bacteria, the zinc ions will combine with the active proteases in the bacteria, thereby causing the bacteria to lose their activity, thereby achieving a sterilization effect. In addition, zinc ions can also enhance the formation of aerogels.
[0009] In addition, when the insulation layer plaster is applied to the steel bar layer, compared with the direct use of zinc ion compounds, the use of nano-metal zinc can promote the formation of a zinc protective layer on the surface of the steel bar, and then obtain cathodic protection through sacrificial anodes to provide antioxidant protection for the steel bar, effectively reducing the possibility of corrosion of the steel bar.
[0010] However, metallic zinc itself does not have antibacterial properties, and if metallic zinc is converted into zinc ion compounds in large quantities, the possibility of steel bar oxidation will increase. Nano-titanium dioxide also has extremely good antibacterial properties. Its antibacterial mechanism is that titanium dioxide is activated by light, generating interactions between electron holes, oxygen molecules, and hydroxide ions, which stimulate free radicals to cause chain reactions, destroy bacterial proteins, and thus achieve a sterilization effect.
[0011] Therefore, when titanium dioxide is mixed with metallic zinc, the insulation layer plaster not only has stable antibacterial and mildew-proof properties, but can also effectively reduce the possibility of oxidation of steel bars or other iron objects.
[0012] In addition, due to the addition of nano-titanium dioxide and nano-metal zinc, the surface of the antibacterial aerogel will form an uneven interface, thereby increasing the contact angle of the antibacterial aerogel surface, thereby obtaining hydrophobic properties, effectively reducing the antibacterial aerogel's absorption of water, and prompting the moisture on the insulation layer plaster to evaporate quickly, effectively reducing the humidity of the insulation layer plaster, and indirectly reducing the possibility of bacterial reproduction.
[0013] Preferably, in the antibacterial hydrophobic aerogel, the molar ratio of nano titanium dioxide to nano metal zinc is 2:(2-3).
[0014] When nano titanium dioxide and nano metal zinc are in the above molar ratio, the thermal insulation layer plaster not only has stable antibacterial and mildew-proof properties, but also can effectively reduce the possibility of oxidation of steel bars or other iron objects.
[0015] Preferably, the antibacterial aerogel is prepared from tetraethyl orthosilicate, octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, acid, alkali, nano titanium dioxide, nano metal zinc and water.
[0016] The octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution contains quaternary ammonium salt and chitosan at the same time.
[0017] Among them, the antibacterial mechanism of quaternary ammonium salts is that quaternary ammonium salts can be adsorbed on the surface of bacteria, thereby changing the permeability of the bacterial cell membrane, causing the enzymes, coenzymes and intermediate metabolites in the bacteria to overflow, hindering the bacterial respiration and glycolysis process, and denaturing bacterial proteins, thereby achieving a bactericidal effect.
[0018] The antibacterial mechanism of chitosan is that chitosan can be adsorbed on the surface of bacterial cells to form a polymer film, thereby preventing nutrients from being transported into the cells, thus achieving an antibacterial and bactericidal effect. At the same time, chitosan can also penetrate into the bacterial cells, thereby adsorbing the anionic cytoplasm in the cells, and then flocculating, disrupting the normal physiological activities of the cells, and then killing bacteria.
[0019] In summary, due to the different antibacterial mechanisms of quaternary ammonium salts, chitosan, titanium dioxide and zinc ion compounds, the addition of octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution can further improve the antibacterial properties of the insulation layer plaster.
[0020] In addition, there is a methyl group in octyldecyl dimethyl ammonium chloride, and the methyl group is a hydrophobic group, which further improves the hydrophobicity of the antibacterial aerogel, promotes the rapid evaporation of moisture on the plaster of the insulation layer, effectively reduces the humidity of the plaster of the insulation layer, and indirectly reduces the possibility of bacterial reproduction.
[0021] In addition, since chitosan has many hydroxyl groups, chitosan can provide a large number of active sites, so it can act as a skeleton support to participate in the formation of the entire network structure of the antibacterial aerogel, further improving the stability of the aerogel.
[0022] Preferably, the antibacterial aerogel is obtained by mixing component A and component B, and the volume ratio of component A to component B is 1:(0.5-1);
[0023] The component A is obtained by mixing ethyl orthosilicate, octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, acid, water, nano titanium dioxide and nano metal zinc; the component B is obtained by mixing octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, alkali and water.
[0024] When preparing the antibacterial aerogel, all components of the antibacterial aerogel are divided into component A and component B, wherein the acid, nano titanium dioxide and nano metal zinc belong to component A, and the base belongs to component B.
[0025] In component A, the acid mainly plays the role of catalyzing hydrolysis, creating an environment that facilitates the sol-gel reaction and controls the pH value of the environment. In addition, the acid can also convert part of the nano-metal zinc into zinc salt, thereby extracting the zinc ions.
[0026] In component B, the alkali is mainly used to further stabilize the aerogel network structure. At the same time, the alkali can also form a precipitate with zinc salt, and zinc hydroxide contains both zinc ions and hydroxide, thereby obtaining excellent antibacterial properties.
[0027] Preferably, in the component A, the molar ratio of the tetraethyl orthosilicate, octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, acid, water, nano titanium dioxide and nano metal zinc is 1: (10-20): (2.4-3.6): (6-8): 10: (10-15);
[0028] In the B component, the molar ratio of the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, alkali and water is 10: (6-8): (0.24-0.36): (0.3-2.7).
[0029] When the raw materials of component A and component B adopt the above molar ratio, the acid can more stably and effectively catalyze the hydrolysis of ethyl orthosilicate and effectively extract zinc ions. The alkali can effectively stabilize the aerogel structure and stably form zinc hydroxide, effectively improving the antibacterial properties of the insulation layer plaster.
[0030] Preferably, the method for preparing the antibacterial aerogel comprises the following steps:
[0031] Preparation of component A: First, nano titanium dioxide and nano zinc are added to the acid and mixed and stirred, then ethyl orthosilicate and water are slowly added, and then mixed and stirred for 2-3 hours, and finally octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution is added, and mixed again for 1-2 hours to obtain component A;
[0032] Component B: Mix and stir octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, alkali and water for 1-3 hours to obtain component B;
[0033] Preparation of antibacterial aerogel: Component B is slowly added to component A, followed by mixing and stirring for 1-2 hours at a temperature of 200-250°C and a pressure of 8-12Mpa, and finally calcined and dried to obtain antibacterial aerogel.
[0034] Preferably, the preparation method of the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution is: dissolving chitosan in acid, then adding octyldecyl dimethyl ammonium chloride to mix, and finally adding ethanol until the solution is completely dissolved.
[0035] Chitosan is insoluble in water, alkali and general organic solvents, but it is soluble in dilute inorganic acid or organic acid. Therefore, when preparing the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, chitosan is first dissolved in acid. However, octyldecyl dimethyl ammonium chloride is soluble in organic solvents, and then octyldecyl dimethyl ammonium chloride and chitosan are effectively blended.
[0036] Preferably, the acid is one of oxalic acid, acetic acid and phosphoric acid, and the base is one of ammonia water, monoethanolamine and diethanolamine.
[0037] Compared with strong acids and bases, weak acids such as oxalic acid, acetic acid, phosphoric acid and weak bases such as ammonia, monoethanolamine, and diethanolamine can more stably catalyze hydrolysis, extract zinc ions, and stabilize the aerogel structure, further improving the antibacterial properties of the insulation layer plaster.
[0038] In a second aspect, the present application provides a method for preparing a thermal insulation layer plastering gypsum, using the following technical solution:
[0039] A method for preparing a thermal insulation layer plastering gypsum comprises the following steps:
[0040] S1. Ball-milling and drying gypsum powder, lightweight filler and antibacterial aerogel;
[0041] S2. Repeatedly mix gypsum powder, alkaline agent, water-retaining agent, retarder, thixotropic agent, air-entraining agent, lightweight filler and antibacterial aerogel to obtain thermal insulation layer plaster.
[0042] In summary, this application has the following beneficial effects:
[0043] 1. When titanium dioxide is mixed with metallic zinc, the insulation layer plaster not only has stable antibacterial and mildew-proof properties, but can also effectively reduce the possibility of oxidation of steel bars or other iron objects.
[0044] 2. The addition of nano titanium dioxide and nano metal zinc will cause the surface of the antibacterial aerogel to form an uneven interface, thereby obtaining hydrophobic properties, which will enable the moisture on the plaster of the insulation layer to evaporate quickly, indirectly reducing the possibility of bacterial reproduction.
[0045] 3. There is also a methyl group in octyldecyl dimethyl ammonium chloride, and the methyl group is a hydrophobic group, which further improves the hydrophobicity of the antibacterial aerogel, promotes the rapid evaporation of the moisture on the plaster of the insulation layer, effectively reduces the humidity of the plaster of the insulation layer, and indirectly reduces the possibility of bacterial reproduction.
[0046] 4. Chitosan has many hydroxyl groups, so chitosan can provide a large number of active sites, which can act as a skeleton support to participate in the formation of the entire network structure of the antibacterial aerogel, further improving the stability of the aerogel. DETAILED DESCRIPTION
[0047] The present application is further described in detail below with reference to examples and comparative examples.
[0048] raw material
[0049] Gypsum powder CAS: 10101-41-4; Alkaline agent - calcium hydroxide CAS: 1305-62-0; Water retention agent - methyl cellulose CAS: 9004-67-5; Retarder - citric acid CAS: 77-92-9; Thixotropic agent OPTIBENT@987; Air entraining agent - AY-02; Lightweight filler - expanded perlite CAS: 93763-70-3; Nano titanium dioxide HTR-616; Nano metal zinc Qiyue Biological 100nm; Tetraethyl orthosilicate CA S: 78-10-4; Octyldecyl dimethyl ammonium chloride CAS: 32426-11-2; Methyltrimethoxysilane CAS: 1185-55-3; Ethanol CAS: 64-17-5; Oxalic acid CAS: 144-62-7; Acetic acid CAS: 127-09-03; Phosphoric acid CAS: 7664-38-2; Ammonia CAS: 13767-16-3; Monoethanolamine CAS: 141-43-5; Diethanolamine CAS: 111-42-2.
[0050] Example
[0051] Example 1
[0052] A thermal insulation layer plastering gypsum comprises 85kg of gypsum powder, 2kg of alkaline agent, 0.2kg of water retaining agent, 0.06kg of retarder, 0.03kg of thixotropic agent, 0.03kg of air entraining agent, 8kg of lightweight filler and 8kg of antibacterial aerogel.
[0053] A method for preparing a thermal insulation layer plaster comprises the following steps:
[0054] S1. Ball-milling and drying gypsum powder, lightweight filler and antibacterial aerogel;
[0055] S2. Repeatedly mix gypsum powder, alkaline agent, water-retaining agent, retarder, thixotropic agent, air-entraining agent, lightweight filler and antibacterial aerogel to obtain thermal insulation layer plaster.
[0056] The antibacterial aerogel is formed by mixing component A and component B, and the volume ratio between component A and component B is 1:(0.5-1). In this embodiment, 1:0.75 is taken as an example for description.
[0057] Component A is obtained by mixing tetraethyl orthosilicate, octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, acid, water, nano titanium dioxide and nano metal zinc, and the molar ratio of tetraethyl orthosilicate, octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, acid (oxalic acid, acetic acid, phosphoric acid are all suitable, oxalic acid is used as an example), water, nano titanium dioxide and nano metal zinc is 1:15:3:7:10:13.
[0058] Component B is obtained by mixing octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, a base (ammonia water, monoethanolamine, diethanolamine are all suitable, ammonia water is used as an example) and water, and the molar ratio of octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, a base and water is 10:7:0.3:1.5.
[0059] The preparation method of antibacterial aerogel comprises the following steps:
[0060] Preparation of component A: First, add nano titanium dioxide and nano metal zinc to the acid, then mix and stir for 1 hour at room temperature and pressure, then slowly add tetraethyl orthosilicate and water, then mix and stir for 2.5 hours (preferably 2-3 hours), finally add octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, and mix again for 1.5 hours (preferably 1-2 hours) to obtain component A;
[0061] Component B: Mix octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, alkali and water and stir for 1.5 hours (preferably 1-3 hours) to obtain component B;
[0062] Preparation of antibacterial aerogel: slowly add component B to component A, then mix and stir for 1.5h (preferably 1-2h) at a temperature of 230°C (preferably 200-250°C) and a pressure of 10Mpa (preferably 8-12Mpa), and finally calcine and dry to obtain antibacterial aerogel.
[0063] The preparation method of octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution is as follows: chitosan is added to excess oxalic acid, and when the chitosan is completely dissolved, octyldecyl dimethyl ammonium chloride is added for mixing, the molar ratio of chitosan to octyldecyl dimethyl ammonium chloride is 1:1, and finally ethanol is added until the octyldecyl dimethyl ammonium chloride is completely dissolved, and when the pH value of the solution reaches 6, the addition of ethanol is stopped.
[0064] Example 2-3
[0065] The difference from Example 1 is that the addition amounts of the components of the thermal insulation layer plaster are different, as shown in Table 1.
[0066] Table 1 Addition amount of each component of the thermal insulation layer plastering gypsum in Examples 1-3 / kg
[0067] Example 1 Example 2 Example 3 Gypsum powder 85 90 80 Alkaline agent 2 1 3 Water Retention Agent 0.2 0.3 0.1 Retarder 0.06 0.10 0.02 Thixotropic agent 0.03 0.02 0.04 Air Entraining Agent 0.03 0.02 0.04 Lightweight filler 8 5 10 Antibacterial aerogel 8 10 5
[0068] Embodiment 4-5
[0069] The difference from Example 1 is that the molar ratio of nano titanium dioxide to nano metal zinc is different, as shown in Table 2.
[0070] Table 2 Molar ratio of nano titanium dioxide to nano metal zinc in Example 1, Example 4-5
[0071] Example 1 Example 4 Example 5 Nano Titanium Dioxide 10 10 10 Nano-metal zinc 13 10 15
[0072] Example 6
[0073] The difference from Example 1 is that, when preparing the antibacterial aerogel, nano titanium dioxide and nano metal zinc are placed in the B component.
[0074] Example 7
[0075] The difference from Example 1 is that oxalic acid is replaced by a hydrochloric acid solution of the same molar amount, and ammonia water is replaced by a sodium hydroxide solution of the same molar amount.
[0076] Example 8
[0077] The difference from Example 1 is that when preparing the antibacterial aerogel, the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution is no longer added.
[0078] Example 9
[0079] The difference from Example 1 is that when preparing the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, octyldecyl dimethyl ammonium chloride is no longer added.
[0080] Example 10
[0081] The difference from Example 1 is that chitosan is no longer added when preparing the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution.
[0082] Examples 11-12
[0083] The difference from Example 1 is that the molar ratios of the components of the antibacterial aerogel are different, as shown in Table 3.
[0084] The component A is obtained by mixing ethyl orthosilicate, octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, acid, water, nano titanium dioxide and nano metal zinc; the component B is obtained by mixing octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, alkali and water.
[0085] Table 3 Molar ratio of each component of the antibacterial aerogel of Example 1 and Examples 11-12
[0086]
[0087]
[0088] Comparative Example
[0089] Comparative Example 1
[0090] The difference from Example 1 is that no antibacterial aerogel is added.
[0091] Comparative Example 2
[0092] The difference from Example 1 is that when preparing the antibacterial aerogel, ethyl orthosilicate and methyltrimethoxysilane are no longer added.
[0093] Comparative Example 3
[0094] The difference from Example 1 is that when preparing the antibacterial aerogel, nano titanium dioxide and nano metal zinc are no longer added.
[0095] Performance testing
[0096] Detection Methods
[0097] 1. Antibacterial Test
[0098] Sample preparation: First, Examples 1-12 and Comparative Examples 1-3 were stirred and mixed with water at a powder-water ratio of 4:1, and then the samples were smoothed to a thickness of 5 mm, and finally cured to obtain thermal insulation layer plaster gypsum samples.
[0099] Test bacteria: Aspergillus niger ATCC16404
[0100] The specific steps are as follows: First, take three 10cm*10cm samples from Examples 1-12 and Comparative Examples 1-3, respectively, and then sterilize the samples with ethanol and dry them. Then dilute 100g of the strain with 1L of sterile water to make a bacterial suspension for use. Take 50ml of deionized water and spray it evenly on the sample surface, then drop 30ml of the bacterial suspension evenly on the sample surface. Then culture it at 37℃ for 24h and observe the results. The negative control is replaced by a sterile plate, and the other operations are the same.
[0101] Finally, the antibacterial rate was calculated, antibacterial rate = (1-current colony content / original colony content) * 100%. Each example or comparative example was tested three times and the average value was taken.
[0102] Test data: The test data of Examples 1-12 and Comparative Examples 1-3 are shown in Table 4.
[0103] Table 4 Test data table of Examples 1-12 and Comparative Examples 1-3
[0104] Antibacterial rate% Antibacterial rate% Example 1 99.6% Example 9 95.3% Example 2 98.4% Example 10 95.0% Example 3 97.5% Embodiment 11 98.5% Example 4 99.2% Example 12 98.2% Example 5 99.6% Comparative Example 1 40.8% Example 6 89.4% Comparative Example 2 94.6% Example 7 96.6% Comparative Example 3 67.2% Example 8 94.1%
[0105] Referring to Example 1 and Comparative Example 1 and combining with Table 4, it can be seen that the antibacterial rate of Comparative Example 1 is significantly reduced compared with that of Example 1, which shows that the antibacterial aerogel can significantly improve the antibacterial effect of the insulation layer plaster.
[0106] Referring to Example 1 and Comparative Example 2 and combining with Table 4, it can be seen that the antibacterial rate of Comparative Example 2 is slightly lower than that of Example 1, which shows that the aerogel itself also has a certain antibacterial effect. The reason is that the porous structure of the aerogel itself can adsorb formaldehyde, and formaldehyde can react with the amino group of bacterial protein or the thiol group in the bacterial enzyme system to undergo nucleophilic addition reaction, so that the bacteria lose their replication ability and cause metabolic system disorder, thereby achieving the purpose of bactericidal and antibacterial.
[0107] Referring to Example 1 and Comparative Example 3 and combining with Table 4, it can be seen that the antibacterial rate of Comparative Example 3 is significantly reduced compared with that of Example 1, which shows that titanium dioxide and zinc oxide have significant antibacterial properties.
[0108] Referring to Examples 1-3 and combining with Table 4, it can be seen that, compared with Example 1, the antibacterial properties of Examples 2-3 are significantly reduced. The reason is that the proportion of antibacterial aerogel in Examples 2-3 is relatively reduced.
[0109] With reference to Example 1, Examples 4-5 and Table 4, it can be seen that the antibacterial rate of Example 4 is slightly decreased compared with Example 1, while the antibacterial rate of Example 5 is substantially unchanged. The reason for this is that the content of nano-metal zinc in Example 5 is too much, and the amount of oxalic acid is insufficient to form new zinc salts. In Example 4, the content of nano-metal zinc is too little, and the generation of zinc salts hinders the contact between acid and nano-metal zinc, thereby reducing the yield of zinc ion compounds and further reducing the antibacterial effect.
[0110] Referring to Example 1 and Example 6 and combining with Table 4, it can be seen that the antibacterial rate of Example 6 is significantly reduced compared with Example 1, which shows that the operation of placing nano-titanium dioxide and nano-metal zinc in component B will significantly reduce the antibacterial performance of the thermal insulation layer plaster. The reason is that when nano-titanium dioxide and nano-metal zinc are placed in component B, nano-titanium dioxide and nano-metal zinc first react with alkali to generate [Zn(OH)4] 2- , which results in the inability to stably produce zinc ions, thereby reducing the antibacterial properties of the insulation layer plaster.
[0111] Referring to Example 1 and Example 7 and combining with Table 4, it can be seen that the antibacterial rate obtained in Example 7 is slightly lower than that in Example 1, which shows that weak acid and weak base can be more conducive to the formation of antibacterial aerogel.
[0112] Referring to Example 1 and Example 8 and combining with Table 4, it can be seen that the antibacterial rate of Example 8 is significantly reduced compared with Example 1, which shows that the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution can effectively improve the antibacterial properties of the insulation layer plaster.
[0113] With reference to Examples 8-10 and in combination with Table 4, it can be seen that, relative to Example 8, the antibacterial rates of Examples 9-10 are slightly improved, which indicates that chitosan and octyldecyl dimethyl ammonium chloride both have certain antibacterial effects.
[0114] With reference to Example 1, Examples 11-12 and in combination with Table 4, it can be seen that relative to Example 1, the antibacterial rates of Examples 11-12 are slightly reduced, which indicates that when the components of the antibacterial aerogel adopt the molar ratio of Example 1, the thermal insulation layer plaster has better antibacterial properties.
[0115] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A thermal insulation layer plastering gypsum, characterized in that: The invention is composed of the following raw materials in parts by weight: 80-90 parts of gypsum powder, 1-3 parts of alkaline agent, 0.1-0.3 parts of water retaining agent, 0.02-0.10 parts of retarder, 0.02-0.04 parts of thixotropic agent, 0.02-0.04 parts of air entraining agent, 5-10 parts of lightweight filler and 5-10 parts of antibacterial aerogel, wherein the antibacterial aerogel contains nano titanium dioxide and nano metal zinc, and a small amount of zinc ion compound is formed on the surface of the nano metal zinc; In the antibacterial aerogel, the molar ratio of nano titanium dioxide to nano metal zinc is 2:(2-3); The antibacterial aerogel is obtained by mixing component A and component B, and the volume ratio of component A to component B is 1:(0.5-1); The component A is obtained by mixing tetraethyl orthosilicate, octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, acid, water, nano titanium dioxide and nano metal zinc; the component B is obtained by mixing octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyl trimethoxysilane, alkali and water; In the component A, the molar ratio of the tetraethyl orthosilicate, octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, acid, water, nano titanium dioxide and nano metal zinc is 1: (10-20): (2.4-3.6): (6-8): 10: (10-15); In the B component, the molar ratio of the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, alkali and water is 10: (6-8): (0.24-0.36): (0.3-2.7); The preparation method of the antibacterial aerogel comprises the following steps: Preparation of component A: First, nano titanium dioxide and nano zinc are added to the acid and mixed and stirred, then ethyl orthosilicate and water are slowly added, and then mixed and stirred for 2-3 hours, and finally octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution is added, and mixed again for 1-2 hours to obtain component A; Component B: Mix and stir octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution, methyltrimethoxysilane, alkali and water for 1-3 hours to obtain component B; Preparation of antibacterial aerogel: Component B is slowly added to component A, followed by mixing and stirring for 1-2 hours at a temperature of 200-250°C and a pressure of 8-12Mpa, and finally calcined and dried to obtain antibacterial aerogel.
2. The thermal insulation layer plaster according to claim 1, characterized in that: The preparation method of the octyldecyl dimethyl ammonium chloride-chitosan-alcohol solution is: dissolving chitosan in acid, then adding octyldecyl dimethyl ammonium chloride to mix, and finally adding ethanol until the solution is completely dissolved.
3. The thermal insulation layer plaster according to claim 1, characterized in that: The acid is one of oxalic acid, acetic acid and phosphoric acid, and the base is one of ammonia water, monoethanolamine and diethanolamine.
4. A method for preparing the thermal insulation layer plaster according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Ball-milling and drying gypsum powder, lightweight filler and antibacterial aerogel; S2. Repeatedly mix gypsum powder, alkaline agent, water-retaining agent, retarder, thixotropic agent, air-entraining agent, lightweight filler and antibacterial aerogel to obtain thermal insulation layer plaster.