A kind of dextran modified PDMS, preparation method and microfluidic chip

The double-layer structure of PDMS modified by cross-linked dextran solves the problem of hydrophobicity on the surface of PDMS microfluidic chips, improves hydrophilicity and detection capabilities, and achieves higher detection sensitivity and hydrophilic stability.

CN116218002BActive Publication Date: 2024-10-01XIAMEN WIZ BIOTECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211649346.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-10-01
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The hydrophobicity of the existing PDMS microfluidic chip surface leads to poor wetting and affects the separation effect. The existing hydrophilic treatment method has single performance.

Method used

Cross-linked dextran is used to modify the surface of PDMS to form a double-layer structure of dextran-modified PDMS. The surface layer is cross-linked dextran and the bottom layer is cross-linked PDMS. They are combined through chemical grafting methods to enhance hydrophilicity. and detection capabilities.

Benefits of technology

The hydrophilic transformation of the PDMS surface is achieved, which enhances the ability to capture fluorescent microspheres, improves detection sensitivity, and maintains good hydrophilicity and stability through the porous structure and large specific surface area of ​​cross-linked dextran.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004011265370000081
    Figure BDA0004011265370000081
  • Figure BDA0004011265370000091
    Figure BDA0004011265370000091
Patent Text Reader

Abstract

The present application relates to the technical field of microfluidic chips, and specifically provides a dextran-modified PDMS, a preparation method and a microfluidic chip. The dextran-modified PDMS of the present application is composed of a surface layer and a bottom layer, the bottom layer is a cross-linked PDMS, and the surface layer is a cross-linked dextran, which is obtained by reacting PDMS with epoxy groups grafted on the surface with dextran and then performing a cross-linking reaction. The dextran-modified PDMS of the present application has good hydrophilicity and hydrophilic stability, and the cross-linked dextran on the surface has a porous property, which has a good separation effect on microspheres and proteins, and can replace the existing PDMS material in microfluidic chips.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of microfluidic chips, and in particular to a dextran-modified PDMS, a preparation method and a microfluidic chip. Background Art

[0002] Polydimethylsiloxane (PDMS) has the characteristics of high transparency, good biocompatibility, good flexibility, high gas permeability, and easy processing, and has become one of the most important main materials for microfluidic chips. However, PDMS also has the disadvantage of surface hydrophobicity, and microfluidic chips are usually used for the analysis and treatment of biologically active substances. Water is generally used as a solvent, so there is a problem of poor wetting, which affects the separation effect. Various methods have been proposed in the prior art to hydrophilize the PDMS surface. These methods mainly solve the problem of hydrophobicity on the PDMS surface and form a hydrophilic surface, but lack additional performance. Summary of the invention

[0003] Dextran has good biocompatibility. Gels made from cross-linked dextran are often used for biochemical separations, such as column chromatography, because of their porous structure.

[0004] In order to solve the problem of single hydrophilic treatment performance of PDMS surface in the prior art, the inventors of this application, after a lot of analysis, experiments and research, used cross-linked dextran to modify the surface of PDMS to obtain dextran-modified PDMS, which has more properties as the main material of microfluidic chips. To this end, this application provides a dextran-modified PDMS, a preparation method and a microfluidic chip.

[0005] This application adopts the following technical solutions:

[0006] A dextran-modified PDMS consists of a surface layer and a bottom layer, wherein the bottom layer is cross-linked PDMS and the surface layer is cross-linked dextran.

[0007] Preferably, the thickness of the bottom layer is 30 μm-2 mm.

[0008] Preferably, the thickness of the surface layer is 1-300 μm.

[0009] A method for preparing dextran-modified PDMS according to any of the above technical solutions comprises the following steps:

[0010] S1, dissolving dextran in a first solvent to obtain a dextran solution;

[0011] S2, immersing the cross-linked PDMS with epoxy group surface modification into the dextran solution described in step S1, adding an alkaline catalyst, reacting for 12-120 hours, washing, and drying to obtain a first modified PDMS;

[0012] S3, soaking the first modified PDMS in step S2 in a second solvent, adding a cross-linking agent to carry out a cross-linking reaction, washing, and drying to obtain the dextran-modified PDMS.

[0013] Preferably, the concentration of the dextran solution in step S1 is 0.5-10 wt %.

[0014] Preferably, the alkaline catalyst in step S2 is selected from one or more of 4-dimethylaminopyridine, triethylamine, N-methyldiethylamine, N-n-propyldiethylamine, N-isopropyldiethylamine and N,N-dimethylaniline.

[0015] Preferably, the first solvent in step S1 and the second solvent in step S3 are independently selected from one or more of water, DMSO, DMF and DMAc.

[0016] Preferably, the cross-linking agent in step S3 is selected from one or more of epichlorohydrin, polyacrylate compounds and polythiol compounds.

[0017] Preferably, in step S3, the weight ratio of the first modified PDMS to the cross-linking agent is 1:0.0005-0.1.

[0018] A microfluidic chip uses the dextran-modified PDMS described in any of the above technical solutions or the dextran-modified PDMS obtained by the preparation method described in any of the above technical solutions as a main material or one of the main materials.

[0019] In summary, this application has the following beneficial effects:

[0020] 1. The dextran-modified PDMS of the present application has a double-layer structure, with the surface layer being cross-linked dextran and the bottom layer being cross-linked PDMS. It combines the characteristics of the two materials, cross-linked dextran and PDMS, and is used in microfluidic chips. It can not only change the PDMS surface from hydrophobic to hydrophilic, but also give play to the characteristics of the porous structure and large specific surface area of ​​cross-linked dextran, and can fix antibodies therein, thereby increasing the probability of capturing fluorescent microspheres and improving the sensitivity of detection.

[0021] 2. The dextran-modified PDMS of the present application, the cross-linked dextran and the cross-linked PDMS are combined by a chemical grafting method, and have strong binding force and high stability.

[0022] 3. In the present application, dextran macromolecules are grafted onto the surface of cross-linked PDMS by reacting dextran with cross-linked PDMS modified with epoxy groups, and then the dextran is cross-linked to obtain dextran gel, which is then dried to obtain dextran-modified PDMS. The preparation method is simple.

[0023] 4. The dextran-modified PDMS of the present application is applied to a microfluidic chip, and the cross-linked dextran is in contact with the detection fluid. It is found that compared with the uncross-linked dextran, the cross-linked dextran has better hydrophilicity and more lasting hydrophilicity, probably due to the porous structure and large specific surface area of ​​the cross-linked dextran. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below.

[0025] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.

[0026] In a first aspect, the present application proposes a dextran-modified PDMS, which consists of a surface layer and a bottom layer, wherein the bottom layer is cross-linked PDMS and the surface layer is cross-linked dextran.

[0027] In this application, the surface layer and the bottom layer are relative concepts, which do not mean that the surface layer must be on the top and the bottom layer must be on the bottom in terms of orientation. In this application, when the dextran-modified PDMS is in contact with a medium (such as a liquid or a solid), the surface layer is in direct contact with the medium, while the bottom layer is not in direct contact with the medium, or in other words, the surface layer is located between the medium and the bottom layer.

[0028] In the preferred technical solution of the present application, the thickness of the bottom layer is 30 μm-2 mm. Furthermore, the thickness of the bottom layer is 50 μm-1.5 mm. In the present application, the thickness of the bottom layer can be set as required, which is a conventional operation in the art.

[0029] In the preferred technical solution of the present application, the thickness of the surface layer is 1-300 μm. Furthermore, the thickness of the surface layer is 5-150 μm. Furthermore, the thickness of the surface layer is 5-100 μm.

[0030] Still further preferably, the thickness of the surface layer does not exceed the thickness of the bottom layer. For example, the thickness of the surface layer may be 1 / 10, 1 / 20, 1 / 30, 1 / 40 or 1 / 50 of the thickness of the bottom layer.

[0031] The second aspect of the present application proposes a method for preparing dextran-modified PDMS as described in any of the above technical solutions, comprising the following steps:

[0032] S1, dissolving dextran in a first solvent to obtain a dextran solution;

[0033] S2, immersing the cross-linked PDMS with epoxy group surface modification into the dextran solution described in step S1, adding an alkaline catalyst, reacting for 12-120 hours, washing, and drying to obtain a first modified PDMS;

[0034] S3, soaking the first modified PDMS in step S2 in a second solvent, adding a cross-linking agent to carry out a cross-linking reaction, washing, and drying to obtain the above-mentioned dextran-modified PDMS.

[0035] In the preferred technical solution of the present application, the concentration of the dextran solution in step S1 is 0.5-10 wt %. Further preferably, the concentration of the dextran solution is 1-5 g / L.

[0036] There have been many reports on cross-linked PDMS modified with epoxy groups. Generally, polar groups such as hydroxyl and carboxyl are introduced on the surface of cross-linked PDMS by plasma or oxidation, and then react with epoxy silane coupling agents (such as KH-560, KH-186, etc.), that is, epoxy groups are grafted on the surface of cross-linked PDMS.

[0037] In the preferred technical solution of the present application, the alkaline catalyst in step S2 is selected from one or more of 4-dimethylaminopyridine, triethylamine, N-methyldiethylamine, N-n-propyldiethylamine, N-isopropyldiethylamine and N,N-dimethylaniline. The alkaline catalyst can catalyze the ring-opening reaction between the hydroxyl groups on the glucose unit in the glucan structure and the epoxy groups on the surface of the cross-linked PDMS, so that the glucan is grafted to the surface of the cross-linked PDMS.

[0038] In the present application, the average relative molecular weight of dextran is not particularly limited, and may be 1000-100000, or further, the average relative molecular weight is 5000-50000. If the molecular weight of dextran is too low, the strength of the surface cross-linked dextran formed will be low, and if the molecular weight of dextran is too large, the reactivity with the cross-linked PDMS surface will be poor. In addition, in the present application, dextran may be unmodified dextran, or dextran modified with carbon-carbon unsaturated double bonds, such as (methyl) acrylate modified dextran and vinyl modified dextran. (Meth) acrylate modified dextran and vinyl modified dextran can be obtained by reacting the corresponding modifier containing epoxy groups with the hydroxyl group of dextran. For example, (methyl) acrylate modified dextran can be obtained by reacting methyl methacrylate glycidyl ether with dextran under catalysis of alkaline substances. Vinyl-modified dextran can be obtained by reacting allyl glycidyl ether or allyl polyethylene glycol glycidyl ether with dextran under the catalysis of alkaline substances.

[0039] In the preferred technical solution of the present application, the first solvent in step S1 and the second solvent in step S3 are independently selected from one or more of water, DMSO, DMF and DMAc. When the first solvent is water, the hydrophilicity of the cross-linked PDMS modified with epoxy groups on the surface is insufficient, which will affect the wettability of the cross-linked PDMS modified with epoxy groups on the surface of the dextran solution in step S2, and further affect the reaction activity of the epoxy groups with the dextran. Therefore, a small amount of surfactant can be added to the dextran solution. There is no special restriction on the surfactant, such as sodium dodecylbenzene sulfonate, sodium dodecyl sulfonate, sodium dodecyl carboxylate, sodium dodecyl alcohol polyoxyethylene ether sulfate, etc., and the amount can be 0.5-1% of the weight of the dextran, and for example, fluorine surfactant, the amount can be 0.01-0.05% of the weight of the dextran, and for example, silicone surfactant, the amount can be 0.1-0.5% of the weight of the dextran.

[0040] In step S3, when the cross-linking agent is water-soluble, water can be used as the solvent. When the cross-linking agent is water-insoluble or has a low solubility in water and a high solubility in an organic solvent, an organic solvent such as DMSO, DMF, etc. can be used.

[0041] In the present application, the cleaning in step S2 can be performed with deionized water to wash away the unreacted dextran without affecting the cross-linked PDMS. After washing with deionized water, the cleaning can be continued with anhydrous ethanol to wash away the water and facilitate drying. The cleaning in step S3 can be performed with anhydrous ethanol, isopropanol and other more environmentally friendly organic solvents.

[0042] In the preferred technical solution of the present application, the crosslinking agent in step S3 is selected from one or more of epichlorohydrin, polyacrylate compounds and polythiol compounds. When the dextran in step S1 of the present application is unmodified, epichlorohydrin can be used as a crosslinking agent; when the dextran is (meth) acrylate modified dextran, a photoinitiator can be directly added and crosslinked under ultraviolet light, or a crosslinking agent polyacrylate compound can be added, and then crosslinked under the irradiation of the photoinitiator and ultraviolet light; when the dextran is vinyl modified dextran, a crosslinking agent polythiol compound can be added, and crosslinked under the irradiation of the photoinitiator and ultraviolet light.

[0043] In the present application, a multi-acrylate compound refers to a compound containing two or more (meth)acrylate structures in its molecular structure, such as 1,6-hexanediol dimethacrylate, ethylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane triacrylate, ethoxylated (3) trimethylolpropane trimethacrylate, ethoxylated (9) trimethylolpropane trimethacrylate, ethoxylated (15) trimethylolpropane trimethacrylate, pentaerythritol tetramethacrylate, etc.

[0044] In the present application, a polythiol compound refers to a compound containing two or more thiol groups in its molecular structure, such as dimercaptopropanol, 1,3-dimercaptopropane, 1,4-dimercaptobutane, 1,6-dimercaptohexane, 1,8-dimercaptooctane, mercaptopropyl silicone oil, mercaptopropyl polyether silicone oil, bis(2-mercaptoethyl) ether, bis(2-ethoxyethyl) ether, bis(4-mercaptophenyl) ether, terminal mercapto polyether, etc.

[0045] In the preferred technical solution of the present application, the weight ratio of the first modified PDMS and the cross-linking agent in step S3 is 1:0.0005-0.1. Furthermore, the weight ratio of the first modified PDMS and the cross-linking agent is 1:0.001-0.005. Different weight ratios of the first modified PDMS and the cross-linking agent will result in different cross-linking degrees of dextran. The weight ratios of the first modified PDMS and the cross-linking agent are the same, and the cross-linking agents used are different, and the cross-linking degrees of dextran are also different.

[0046] In a third aspect, the present application proposes a microfluidic chip, which uses the dextran-modified PDMS described in any of the above technical solutions or the dextran-modified PDMS obtained by the preparation method described in any of the above technical solutions as the main material or one of the main materials.

[0047] When the dextran-modified PDMS of the present application is used as the main material in a microfluidic chip, the cross-linked dextran can be directly modified on the surface of the molded cross-linked PDMS, and the path through which the liquid flows is changed from PDMS to cross-linked dextran. Due to the hydrophilicity of the cross-linked dextran, the hydrophobic phenomenon of PDMS will not exist.

[0048] The dextran-modified PDMS, preparation method and microfluidic chip of the present application will be described in detail below in combination with examples, comparative examples and experimental data.

[0049] Unless otherwise specified, the parts in the following embodiments and comparative examples are parts by weight.

[0050] Preparation Example 1

[0051] 5 parts of dextran with an average relative molecular weight of 30,000 and 2 parts of 4-dimethylaminopyridine were dissolved in 100 parts of DMSO, glycidyl methacrylate was added (the molar ratio of glycidyl methacrylate to furanose units in dextran was 1:6), and the reaction was stirred at room temperature for 50 hours; the reaction solution was added dropwise to 800 parts of anhydrous ethanol for precipitation, the solid was collected and dried to obtain acrylate-modified dextran.

[0052] Preparation Example 2

[0053] In Preparation Example 1, the molar ratio of glycidyl methacrylate to furanose units in dextran was adjusted from 1:6 to 1:4, and the remaining steps remained unchanged.

[0054] Preparation Example 3

[0055] 4 parts of dextran with an average relative molecular weight of 10,000 and 2 parts of 4-dimethylaminopyridine are dissolved in 100 parts of DMSO, allyl glycidyl ether is added (the molar ratio of allyl glycidyl ether to furanose glucan unit in dextran is 1:5), and the reaction is stirred at room temperature for 48 hours; the reaction solution is added dropwise to 800 parts of anhydrous ethanol for precipitation, the solid is collected and dried to obtain vinyl-modified dextran.

[0056] Preparation Example 4

[0057] 4 parts of dextran with an average relative molecular weight of 10,000 and 2 parts of 4-dimethylaminopyridine are dissolved in 100 parts of DMSO, and glycidyl ether allyl polyoxyethylene ether-200 (200 represents the relative molecular weight of polyoxyethylene) (the molar ratio of glycidyl ether allyl polyoxyethylene ether to the furanose glucan unit in dextran is 1:3) is added, and the reaction is stirred at room temperature for 48 hours; the reaction solution is added dropwise to 800 parts of anhydrous ethanol for precipitation, the solid is collected, and dried to obtain vinyl-modified dextran.

[0058] Preparation Example 5

[0059] In Preparation Example 4, the molar ratio of hydroglyceryl ether allyl polyoxyethylene ether to the furanose glucan unit in glucan was adjusted from 1:3 to 1:6, and the other steps remained unchanged.

[0060] Example 1

[0061] 4 parts of acrylate-modified dextran prepared in Preparation Example 1, 1 part of triethylamine and 0.8 parts of sodium dodecylbenzenesulfonate were added to 94.2 parts of

[0062] Prepare dextran solution in water.

[0063] Add 100mL 1mol / L NaOH aqueous solution and 400mL 30wt% H2O2 to a 1000mL wide-mouth bottle, put a PDMS microfluidic chip substrate with an average thickness of 200μm into the wide-mouth bottle, fix it above the liquid surface, plug the bottle mouth with a rubber stopper equipped with a three-way, keep the three-way open for 2 hours, then close the three-way, and place the wide-mouth bottle in a dark place for 3d. Take it out, seal the substrate with the cover sheet, pass a 5wt% KH-560 ethanol solution into the channel, react at room temperature for 4 hours, rinse the channel with deionized water twice, then pass the above-mentioned dextran solution, react for 48 hours, wash twice, wash once with anhydrous ethanol, and dry at 50°C to obtain the first modified PDMS.

[0064] 100 parts of the first modified PDMS were immersed in 300 parts of DMSO, and 0.15 parts of dimethacrylate 1,6-hexanediol and 0.005 parts of benzoin dimethyl ether were added. 2 The film was irradiated under UV light for 30 s, washed twice with anhydrous ethanol, and dried at 50°C to obtain dextran-modified PDMS.

[0065] Example 2

[0066] In Example 1, the acrylate-modified dextran of Preparation Example 1 was replaced by the acrylate-modified dextran of Preparation Example 2 at an equal concentration, and the other steps remained unchanged.

[0067] Example 3

[0068] 5 parts of the vinyl-modified dextran prepared in Preparation Example 3, 1 part of 4-dimethylaminopyridine and 0.8 parts of sodium dodecylbenzenesulfonate were added to 93.2 parts of water to prepare a dextran solution.

[0069] Add 100mL 1mol / LNaOH aqueous solution and 400mL 30wt% H2O2 to a 1000mL wide-mouth bottle, put a PDMS microfluidic chip substrate with an average thickness of 100μm into the wide-mouth bottle, fix it above the liquid surface, plug the bottle mouth with a rubber stopper equipped with a three-way, keep the three-way open for 2 hours, then close the three-way, and place the wide-mouth bottle in a dark place for 3d. Take it out, seal the substrate with the cover sheet, pass a 3wt% KH-560 ethanol solution into the channel, react at room temperature for 5 hours, rinse the channel with deionized water twice, then pass the above-mentioned dextran solution, react for 54 hours, wash twice, wash once with anhydrous ethanol, and dry at 50°C to obtain the first modified PDMS.

[0070] 100 parts of the first modified PDMS were immersed in 250 parts of water, 0.5 parts of bis(2-ethoxyethyl) ether and 0.005 parts of photoinitiator LAP were added, and the main wavelength was 405nm and the intensity was 10mW / cm 2 The film was irradiated under UV light for 30 s, washed twice with anhydrous ethanol, and dried at 50°C to obtain dextran-modified PDMS.

[0071] Example 4

[0072] In Example 3, the vinyl-modified dextran of Preparation Example 3 was replaced by the vinyl-modified dextran of Preparation Example 4 at an equal concentration, and the other steps remained unchanged.

[0073] Example 5

[0074] In Example 3, the vinyl-modified dextran of Preparation Example 3 was replaced by the vinyl-modified dextran of Preparation Example 5 at an equal concentration, and the other steps remained unchanged.

[0075] Example 6

[0076] 4 parts of the acrylate-modified dextran prepared in Preparation Example 2, 1 part of 4-dimethylaminopyridine and 0.8 parts of sodium dodecyl sulfate were added to 94.2 parts of water to prepare a dextran solution.

[0077] Add 100mL 1mol / LNaOH aqueous solution and 400mL 30wt% H2O2 to a 1000mL wide-mouth bottle, put a PDMS microfluidic chip substrate with an average thickness of 300μm into the wide-mouth bottle, fix it above the liquid surface, plug the bottle mouth with a rubber stopper equipped with a three-way, keep the three-way open for 2 hours, then close the three-way, and place the wide-mouth bottle in a dark place for 3d. Take it out, seal the substrate with the cover sheet, pass an ethanol solution of KH-560 with a concentration of 5wt% into the channel, react at room temperature for 4 hours, rinse the channel with deionized water twice, then pass the above-mentioned dextran solution, react for 48 hours, wash twice, wash once with anhydrous ethanol, and dry at 50℃ to obtain the first modified PDMS.

[0078] 100 parts of the first modified PDMS were immersed in 300 parts of water, and 0.1 parts of polyethylene glycol dimethacrylate-400 (400 represents the molecular weight of polyethylene glycol) and 0.005 parts of benzoin dimethyl ether were added. 2 The film was irradiated under UV light for 30 s, washed twice with anhydrous ethanol, and dried at 50°C to obtain dextran-modified PDMS.

[0079] Example 7

[0080] In Example 6, the weight of polyethylene glycol dimethacrylate-400 was adjusted from 0.1 parts to 0.2 parts, and the other steps remained unchanged.

[0081] Example 8

[0082] In Example 6, the weight of polyethylene glycol dimethacrylate-400 was adjusted from 0.1 parts to 0.3 parts, and the other steps remained unchanged.

[0083] Example 9

[0084] In Example 6, the weight of polyethylene glycol dimethacrylate-400 was adjusted from 0.1 parts to 0.4 parts, and the other steps remained unchanged.

[0085] Example 10

[0086] In Example 6, the weight of polyethylene glycol dimethacrylate-400 was adjusted from 0.1 parts to 0.5 parts, and the other steps remained unchanged.

[0087] Comparative Example 1

[0088] Unmodified PDMS microfluidic chip substrate.

[0089] Comparative Example 2

[0090] The first modified PDMS in Example 8.

[0091] Comparative Example 3

[0092] PDMS that did not react with KH-560 after oxidation in Example 8.

[0093] Comparative Example 4

[0094] In Example 8, the weight of polyethylene glycol dimethacrylate-400 was adjusted from 0.3 parts to 0.03 parts, and the other steps remained unchanged.

[0095] Comparative Example 5

[0096] In Example 8, polyethylene glycol dimethacrylate-400 was not added, and the remaining steps remained unchanged.

[0097] Performance Testing

[0098] Hydrophilicity test: Use the water drop angle to test the water drop angle of the sample to be tested, which is recorded as the initial water drop angle. Along the channel direction, take the front, middle and back three parts for testing. Take the average of the water drop angles of the three parts.

[0099] Hydrophilic stability test. The samples to be tested were baked in a 50°C oven for 7 days and 1 month, respectively, and then taken out and tested according to the above hydrophilic test method, which was recorded as the baked water drop angle. Water drop angle retention rate = water drop angle after baking / initial water drop angle × 100%. The lower the water drop angle retention rate, the better the hydrophilic stability.

[0100] The results are shown in Table 1.

[0101] Table 1

[0102]

[0103]

[0104] Therefore, it can be seen from the data in Table 1 that the dextran-modified PDMS of the present application has good hydrophilicity and lasting hydrophilicity, and can replace the existing PDMS material in the microfluidic chip.

[0105] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A dextran-modified PDMS, characterized in that: It consists of a surface layer and a bottom layer, wherein the bottom layer is cross-linked PDMS and the surface layer is cross-linked dextran; The thickness of the surface layer is 1 / 10, 1 / 20, 1 / 30, 1 / 40 or 1 / 50 of the thickness of the bottom layer. The preparation method of the dextran-modified PDMS comprises the following steps: S1, dissolving acrylate-modified dextran in a first solvent, adding triethylamine and sodium dodecylbenzenesulfonate to obtain an acrylate-modified dextran solution; S2, immersing the cross-linked PDMS with epoxy group surface modification into the dextran solution described in step S1, reacting for 12-120 hours, washing, and drying to obtain a first modified PDMS; S3, immersing the first modified PDMS in step S2 in a second solvent, adding 1,6-hexanediol dimethacrylate and benzoin dimethyl ether, at a main wavelength of 365nm and an intensity of 10mW / cm 2 Irradiating under ultraviolet light to carry out cross-linking reaction, washing, and drying to obtain the dextran-modified PDMS; Wherein, in step S1, the preparation method of acrylate-modified dextran is: 5 parts of dextran with an average relative molecular weight of 30,000 and 2 parts of 4-dimethylaminopyridine are dissolved in 100 parts of DMSO, glycidyl methacrylate is added, and the molar ratio of glycidyl methacrylate to furanose units in dextran is 1:

6. The mixture is stirred and reacted at room temperature for 50 hours; the reaction solution is added dropwise to 800 parts of anhydrous ethanol for precipitation, and the solid is collected and dried to obtain acrylate-modified dextran.

2. The dextran-modified PDMS according to claim 1, characterized in that: The thickness of the bottom layer is 30 μm-2 mm.

3. The dextran-modified PDMS according to claim 1, characterized in that: The thickness of the surface layer is 1-300 μm.

4. The dextran-modified PDMS according to claim 1, characterized in that: The concentration of the dextran solution in step S1 is 0.5-10wt%.

5. The dextran-modified PDMS according to claim 4, characterized in that: The first solvent in step S1 and the second solvent in step S3 are independently selected from one or more of water, DMSO, DMF and DMAc.

6. The dextran-modified PDMS according to claim 4, characterized in that: In step S3, the weight ratio of the first modified PDMS to the 1,6-hexanediol dimethacrylate is 1:0.0005-0.

1.

7. A microfluidic chip, characterized in that: The dextran-modified PDMS according to any one of claims 1 to 3 is used as the main material or one of the main materials.

Citation Information

Patent Citations

  • Polyacrylic ester and polyacrylic ester copolymer material hydrophilic modification products and hydrophilic modification method of polyacrylic ester

    CN102617869A

  • Hyperbranched modified molecular engram polymer and application thereof

    CN102702447A

  • Method to activate silicone rubber surfaces

    CN102782064A

  • Method for modifying polydimethylsiloxane material

    CN112442207A

  • Super-lubricity material as well as preparation method and application thereof

    CN114349996A