Chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material and preparation method thereof
By modifying the filler with chitosan and silane coupling agent, the problem of increased hardness of thermally conductive composite materials when increasing thermal conductivity was solved, and a silicone oil-based flexible thermally conductive composite material with high conductivity and moderate hardness was obtained, which improved the electronic The heat dissipation performance of the device.
Patent Information
- Application Number
- CN202310178350.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-28
AI Technical Summary
It is difficult for existing thermally conductive composite materials to maintain sufficient flexibility while increasing thermal conductivity, resulting in a decrease in fit with electronic components and radiators, affecting heat dissipation efficiency.
Modification of flake and granular fillers by using chitosan and silane coupling agents inhibits the hydrosilylation reaction, reduces composite hardness, and improves the compatibility of fillers in the polymer matrix through silane coupling agents , build a dense heat conduction channel.
The thermal conductivity is increased and the hardness is reduced, and a silicone oil-based flexible thermal composite material with high conductivity and moderate hardness is obtained, which can better fit the surface of electronic components and radiators, and improve the heat dissipation efficiency of electronic equipment.
Smart Images

Figure CN116218231B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of thermal interface materials, and in particular to a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material and a preparation method thereof. Background Art
[0002] At present, electronic components are rapidly developing towards miniaturization, integration, and intelligence. The higher the integration of electronic components, the more heat will be generated during operation, which will inevitably increase the operating temperature of electronic equipment and greatly affect its performance, safety, and service life. Therefore, the preparation of thermal conductive materials with efficient heat dissipation is crucial to the construction of advanced modern microelectronics technology.
[0003] Addition-type liquid silicone rubber is a silicone rubber formed by the silylation reaction of vinyl-terminated silicone oil and hydrogen-containing silicone oil under the action of a catalyst. It is very conducive to industrial production due to its low cost and easy processing. Its excellent flexibility enables it to fit well on the surface of electronic components and radiators, filling the tiny gaps on their surfaces, which is conducive to heat conduction. At the same time, it is widely used in electronic products because of its excellent corrosion resistance, aging resistance and electrical insulation properties. However, the intrinsic thermal conductivity of addition-type liquid silicone rubber is low (0.1-0.2W·m -1 ·K -1 ), which limits its application in the field of heat dissipation of electronic equipment.
[0004] Introducing thermally conductive fillers with high thermal conductivity into the silicone rubber matrix is one of the most effective methods for preparing high thermal conductivity composite materials. However, to prepare thermally conductive composite materials with high thermal conductivity, it is necessary to fill enough thermally conductive fillers to build as many thermal conductive channels as possible in the silicone rubber matrix. While too high a filling rate of thermally conductive fillers will inevitably increase the hardness of the composite material while increasing the thermal conductivity of the composite material, resulting in a lack of flexibility in the material. Therefore, how to obtain a flexible thermally conductive composite material with high thermal conductivity and moderate hardness has become a difficult problem that researchers need to solve.
[0005] For example, Chinese invention patent application CN101812233A discloses a two-component addition room temperature curing silicone rubber, which is prepared by stirring and heating allyl silicone oil, hydrogen silicone oil, aluminum oxide, quartz powder, platinum catalyst, inhibitor and other substances, and has a thermal conductivity of 0.7-1.0 W·m -1 ·K -1 , and the Shore A hardness is between 45 and 64. However, higher hardness will affect the fit between the thermally conductive composite material and the surface of electronic components and radiators, forming larger gaps. A large amount of air with extremely low thermal conductivity will fill the gaps, which will hinder the rapid heat dissipation of electronic equipment. Summary of the invention
[0006] In view of the above situation, the present invention provides a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material with high thermal conductivity and low hardness and a preparation method thereof.
[0007] The present invention uses chitosan and silane coupling agent to modify the flaky filler and the granular filler at the same time, and the flaky filler and the granular filler are organically matched. Chitosan inhibits the silane hydroaddition reaction of terminal vinyl silicone oil and hydrogen-containing silicone oil, reduces the crosslinking between the two monomers, and thus reduces the hardness of the composite material; the grafting of the silane coupling agent on the surface of the thermally conductive filler improves their compatibility in the polymer matrix, reduces the thermal resistance of the filler-matrix interface, the flaky filler is used as the main filler to construct the main thermal conductive path, and the granular filler is used as the auxiliary filler to insert the gap between the flaky fillers, so that the thermal conductive channels in the polymer matrix are more dense, thereby obtaining a chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material with high thermal conductivity and moderate hardness.
[0008] The present invention is achieved through the following technical solutions:
[0009] The chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material is obtained by heating and curing a fluid slurry; the fluid slurry is obtained by uniformly stirring a modified flaky filler and a modified granular filler, a silicone oil mixture and a platinum catalyst and then removing bubbles; the modified flaky filler or modified granular filler is obtained by adding chitosan, a granular filler or a flaky filler to an ethanol aqueous solution, adding glacial acetic acid, stirring evenly, adding a silane coupling agent and stirring, and filtering, washing and drying after the reaction is completed.
[0010] To further achieve the purpose of the present invention, preferably, in terms of mass percentage, the silicone oil mixture accounts for 50-70% of the raw material mass, the modified flaky filler and the modified granular filler account for 30-50% of the raw material mass, of which the flaky filler accounts for 20-40% and the granular filler accounts for 10-20%; the silicone oil mixture is obtained by uniformly stirring terminal vinyl silicone oil, side hydrogen-containing silicone oil and an inhibitor; the mass ratio of terminal vinyl silicone oil to side hydrogen-containing silicone oil is 4:1-5:1; the inhibitor is 0.1-1% of the mass of the mixture of vinyl silicone oil and side hydrogen-containing silicone oil; the amount of platinum catalyst is not included in the total mass percentage of the raw material, and 20-30 μL of platinum catalyst is added to every 10g of the mixture of terminal vinyl silicone oil, side hydrogen-containing silicone oil and inhibitor.
[0011] Preferably, the granular filler is one or more of spherical aluminum oxide, spherical magnesium oxide, aluminum nitride, silicon nitride and silicon carbide; the flaky filler is one or more of flake graphite, hexagonal boron nitride, graphene oxide, graphene and graphene nanosheets.
[0012] Preferably, the viscosity of the chitosan is less than 200 mPa·s, and the amount of chitosan used is 1-2% of the mass of the granular filler and the flaky filler; the volume ratio of deionized water to anhydrous ethanol in the ethanol aqueous solution is 3:1-5:1, the amount of glacial acetic acid used is 1-2 ml per 100 ml of the ethanol aqueous solution, the amount of ethanol aqueous solution used in the modification process of the flaky filler is 200-300 ml of ethanol aqueous solution for every 25 g of filler; the amount of ethanol aqueous solution used in the modification process of the granular filler is 100-150 ml of ethanol aqueous solution for every 25 g of filler.
[0013] Preferably, the silane coupling agent is composed of one or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane and vinyltriethoxysilane.
[0014] Preferably, the usage amount of the silane coupling agent is 1-2% of the mass of the granular filler and the flaky filler, the reaction time after adding the silane coupling agent is 1-3 hours, and the reaction temperature is room temperature.
[0015] Preferably, the vinyl-terminated silicone oil is divinyl-terminated polydimethylsiloxane with a viscosity of 100-500 mPa·s and a vinyl content of 0.30-1.10 wt %; the hydrogen-containing silicone oil is polymethyl hydrogen siloxane with a hydrogen content of 0.1-0.8 wt %.
[0016] Preferably, the inhibitor is ethynyl cyclohexanol, and the catalyst is a Karstedt platinum catalyst, which is a complex formed by zero-valent platinum and divinyltetramethyldisiloxane, and the concentration of zero-valent platinum in the catalyst is 1000-5000 ppm. More preferably, the concentration of zero-valent platinum is 3000 ppm.
[0017] The method for preparing the chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material comprises the following steps:
[0018] (1) adding the chitosan, granular filler or flake filler to an ethanol aqueous solution, adding glacial acetic acid, stirring evenly, adding a silane coupling agent and stirring after the mixture is evenly mixed, and filtering after the reaction is completed, washing with deionized water and vacuum drying to obtain a modified flake filler or a modified granular filler;
[0019] (2) mixing the vinyl-terminated silicone oil, the hydrogen-containing silicone oil and the inhibitor to obtain a silicone oil mixture;
[0020] (3) adding the modified flaky filler and the modified granular filler obtained in step (1), the silicone oil mixture obtained in step (2), and the platinum catalyst into a container, stirring evenly to obtain a fluid slurry;
[0021] (4) degassing the fluid slurry and injecting it into a mold;
[0022] (5) heating and curing to form, and demolding after cooling to room temperature to obtain a silicone oil-based flexible thermal conductive composite material modified with chitosan and silane coupling agent.
[0023] Preferably, in step (1), the stirring conditions before and after adding the silane coupling agent are a rotation speed of 500 to 800 rpm, a temperature of room temperature, and a stirring time of 1 to 2 hours; the vacuum drying temperature is 80 to 100° C., the vacuum degree is -0.08 to -0.10 MPa, and the vacuum drying time is 12 to 24 hours;
[0024] In step (2), the stirring is performed at room temperature, the stirring speed is 400 to 600 rpm, and the stirring time is 2 to 6 hours;
[0025] In step (3), the stirring is performed at room temperature, the stirring speed is 600 to 1000 rpm, and the stirring time is 0.5 to 2 h;
[0026] In step (4), the degassing is performed by placing the fluid slurry in a vacuum drying oven for vacuum degassing; the vacuum degassing is performed at room temperature and a vacuum degree of -0.10 MPa for 0.5 to 1 h;
[0027] In step (5), the heating and curing molding is to place the slurry together with the mold in a blast dryer for heating to solidify the material; the heating temperature of the blast dryer is 60-80°C and the heating time is 1-2h.
[0028] Compared with the prior art, the advantages and beneficial technical effects of the present invention are:
[0029] 1) The present invention uses chitosan and a silane coupling agent to modify the thermally conductive filler, so that when the filler filling mass fraction of the thermally conductive composite material is high, the hardness of the thermally conductive composite material is significantly reduced compared with that before modification, and at the same time, the thermal conductivity is greatly improved, which effectively solves the problem that it is difficult to achieve both high thermal conductivity and appropriate hardness of the thermally conductive composite material.
[0030] 2) The flaky filler of the present invention is used as the main filler with a mass fraction of 20-40%, and the granular filler is used as the auxiliary filler with a mass fraction of 10-20%, and the total filling mass fraction of the two fillers is 30-50%; the flaky filler is used as the main filler to construct the main heat conduction path, and the granular filler is used as the auxiliary filler to be inserted into the gaps between the flaky fillers, so that the heat conduction channels in the polymer matrix are more dense.
[0031] 3) The thermal conductivity of the chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material obtained by the present invention can reach up to 1.309 W·m -1 ·K -1 , while the Shore hardness A is the lowest at 34.5. The Shore hardness A of the material prepared using fillers modified with chitosan (CTS) and silane coupling agents is around 35-40, and the hardness decreases by more than 25% compared with the material prepared using unmodified fillers. This may be because chitosan inhibits the silylation reaction of terminal vinyl silicone oil and hydrogen-containing silicone oil, and reduces the crosslinking between the two monomers. Compared with the material prepared using unmodified fillers, the thermal conductivity of the chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material obtained by the present invention is increased by 8-10%, which may be because the grafting of silane coupling agents on the filler surface improves the compatibility of the filler in the matrix and reduces the phonon scattering of the filler-matrix interface. At the same time, the combined use of the two types of fillers also produces a positive effect.
[0032] 4) Under the condition of the same thermal conductivity, the thermally conductive composite material with lower hardness can better fit the surface of electronic components and radiators, thus being more conducive to the actual heat dissipation of electronic equipment. The chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material of the present invention has higher thermal conductivity and lower hardness, can better fit the surface of electronic components and radiators, and can effectively solve the heat dissipation problem of electronic equipment.
[0033] 5) The present invention does not use toxic or harmful reagents in the thermal conductive filler modification process, is environmentally friendly, has low material costs, and is easy to carry out industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the Fourier transform infrared spectra of the flake graphite before and after modification obtained in Example 1.
[0035] Figure 2 This is the Fourier infrared spectra of the spherical alumina before and after modification obtained in Example 1. DETAILED DESCRIPTION
[0036] In order to better understand the present invention, the present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to the specific embodiments.
[0037] Example 1
[0038] A method for preparing a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material comprises the following steps:
[0039] (1) 0.25 g chitosan (CTS, viscosity <200 mPa·s) and 25 g flake graphite (FG, particle size 200 mesh) were added to 200 ml ethanol aqueous solution (the volume ratio of ethanol to deionized water was 1:3), and then 2 ml glacial acetic acid was added. The mixture was magnetically stirred at 700 rpm for 2 h at room temperature, and then 0.5 g γ-methacryloxypropyltrimethoxysilane (KH570) was added. The mixture was stirred for 2 h. After filtration and washing with anhydrous ethanol, the mixture was transferred to a vacuum drying oven and dried at 100°C and -0.10 MPa for 12 h to obtain flake graphite modified with chitosan and γ-methacryloxypropyltrimethoxysilane, which was recorded as FG-CTS-KH570.
[0040] Similarly, spherical alumina (S-Al2O3, particle size 50 μm) was modified using the same method as flake graphite modification. The only difference was that in the modification of granular fillers such as spherical alumina, the amount of ethanol aqueous solution was reduced to 100 ml, and the amount of glacial acetic acid was reduced to 1 ml. Finally, spherical alumina modified with chitosan and γ-methacryloxypropyltrimethoxysilane was obtained, which was recorded as Al2O3-CTS-KH570;
[0041] (2) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0042] (3) 12 g and 8 g of FG-CTS-KH570 and Al2O3-CTS-KH570 obtained in step (1) were respectively placed in a container, and 20 g of the silicone oil mixture obtained in step (2) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration of 3000 ppm) were added, and stirred evenly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 hour to obtain a uniform and fluid slurry;
[0043] (4) placing the slurry obtained in step (3) into a vacuum drying oven, degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa, and injecting into a mold after degassing;
[0044] (5) The slurry and the mold are placed in a forced air dryer and heated at 80° C. for 2 h to solidify the slurry. After cooling to room temperature, the slurry is demolded to obtain a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material.
[0045] In Example 1, the filling mass fractions of FG-CTS-KH570 and Al2O3-CTS-KH570 are 30% and 20%, respectively.
[0046] Figure 1 The Fourier transform infrared spectra of FG before and after modification obtained in Example 1 are as follows: Figure 1 As shown, the FG modified by chitosan (CTS) has a wavelength of 3440 cm -1 The stretching vibration peak intensity of the hydroxyl (-OH) group increased, which may be caused by the adsorption of CTS rich in -OH on the FG surface. After the FG was modified with CTS and γ-methacryloxypropyltrimethoxysilane (KH570), the peak at 3440 cm -1 The stretching vibration peak intensity of the hydroxyl group (-OH) is reduced to 1086cm -1 The Si-O-Si infrared characteristic peak appeared at 1161cm -1 The Si-OC infrared characteristic peak appeared, proving that KH570 was successfully grafted onto the FG surface;
[0047] Figure 2 The Fourier transform infrared spectra of S-Al2O3 before and after modification obtained in Example 1 are as follows: Figure 2 As shown in the figure, there is no significant difference in the infrared spectra of Al2O3 before and after CTS modification, which may be caused by the small amount of Al2O3 adsorbed on the surface of CTS. After being modified by CTS and KH570, the Al2O3 has a peak at 1623cm -1 The infrared characteristic peak of carbon-carbon double bond (C=C) appeared, indicating that KH570 was successfully grafted onto the Al2O3 surface.
[0048] Example 2
[0049] A method for preparing a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material comprises the following steps:
[0050] (1) 0.5 g chitosan (CTS, viscosity <200 mPa·s) and 25 g flake graphite (FG, particle size 200 mesh) were added to 200 ml ethanol aqueous solution (the volume ratio of ethanol to deionized water was 1:4), and then 2 ml glacial acetic acid was added. The mixture was magnetically stirred at 700 rpm for 2 h at room temperature, and then 0.25 g vinyltrimethoxysilane (KH171) was added. The mixture was stirred for 2 h. After filtration and washing with anhydrous ethanol, the mixture was transferred to a vacuum drying oven and dried at 100°C and -0.10 MPa for 12 h to obtain flake graphite modified with chitosan and vinyltrimethoxysilane, which was recorded as FG-CTS-KH171.
[0051] Similarly, spherical alumina (S-Al2O3, particle size 50 μm) was modified using the same method, except that for granular fillers such as spherical alumina, the amount of ethanol aqueous solution was reduced to 100 ml, and the amount of glacial acetic acid was reduced to 1 ml. Finally, spherical alumina modified with chitosan and vinyltrimethoxysilane was obtained, which was recorded as Al2O3-CTS-KH171;
[0052] (2) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0053] (3) 12 g and 8 g of FG-CTS-KH171 and Al2O3-CTS-KH171 obtained in step (1) were respectively placed in a container, and 20 g of the silicone oil mixture obtained in step (2) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration of 3000 ppm) were added, and stirred evenly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 hour to obtain a uniform and fluid slurry;
[0054] (4) placing the slurry obtained in step (3) into a vacuum drying oven, degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa, and injecting into a mold after degassing;
[0055] (5) The slurry and the mold are placed in a forced air dryer and heated at 80° C. for 2 h to solidify the slurry. After cooling to room temperature, the slurry is demolded to obtain a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material.
[0056] In Example 2, the filling mass fractions of FG-CTS-KH171 and Al2O3-CTS-KH171 are 30% and 20%, respectively.
[0057] Example 3
[0058] A method for preparing a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material comprises the following steps:
[0059] (1) 0.5 g chitosan (CTS, viscosity <200 mPa·s) and 25 g flake graphite (FG, particle size 200 mesh) were added to 200 ml ethanol aqueous solution (the volume ratio of ethanol to deionized water was 1:5), and then 4 ml glacial acetic acid was added. The mixture was magnetically stirred at 700 rpm for 2 h at room temperature, and then 0.5 g vinyl triethoxysilane (KH151) was added. The mixture was stirred for 2 h. After filtration and washing with anhydrous ethanol, the mixture was transferred to a vacuum drying oven and dried at 100°C and -0.10 MPa for 12 h to obtain flake graphite modified with chitosan and vinyl triethoxysilane, which was recorded as FG-CTS-KH151.
[0060] Similarly, spherical alumina (S-Al2O3, particle size 50 μm) was modified using the same method, except that for granular fillers such as spherical alumina, the amount of ethanol aqueous solution was reduced to 100 ml, and the amount of glacial acetic acid was reduced to 2 ml. Finally, spherical alumina modified with chitosan and vinyl triethoxysilane was obtained, which was recorded as Al2O3-CTS-KH151;
[0061] (2) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0062] (3) 12 g and 8 g of FG-CTS-KH151 and Al2O3-CTS-KH151 obtained in step (1) were respectively placed in a container, and 20 g of the silicone oil mixture obtained in step (2) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration of 3000 ppm) were added, and stirred evenly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 hour to obtain a uniform and fluid slurry;
[0063] (4) placing the slurry obtained in step (3) into a vacuum drying oven, degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa, and injecting into a mold after degassing;
[0064] (5) The slurry and the mold are placed in a forced air dryer and heated at 80° C. for 2 h to solidify the slurry. After cooling to room temperature, the slurry is demolded to obtain a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material.
[0065] In Example 3, the filling mass fractions of FG-CTS-KH151 and Al2O3-CTS-KH151 are 30% and 20%, respectively.
[0066] Example 4
[0067] A method for preparing a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material comprises the following steps:
[0068] (1) 0.375 g of chitosan (CTS, viscosity <200 mPa·s) and 25 g of hexagonal boron nitride (h-BN, particle size 20-30 μm) were added to 200 ml of ethanol aqueous solution (the volume ratio of ethanol to deionized water was 1:3), and then 2 ml of glacial acetic acid was added. The mixture was magnetically stirred at 700 rpm for 2 h at room temperature, and then 0.375 g of γ-glycidyloxypropyltrimethoxysilane (KH560) was added. The mixture was stirred for 2 h. After filtration and washing with anhydrous ethanol, the mixture was transferred to a vacuum drying oven and dried at 100°C and -0.10 MPa for 12 h to obtain hexagonal boron nitride modified with chitosan and γ-glycidyloxypropyltrimethoxysilane, which was recorded as BN-CTS-KH560.
[0069] Similarly, spherical alumina (S-Al2O3, particle size 50 μm) was modified using the same method, except that for granular fillers such as spherical alumina, the amount of ethanol aqueous solution was reduced to 100 ml, and the amount of glacial acetic acid was reduced to 1 ml. Finally, spherical alumina modified with chitosan and γ-glycidyloxypropyltrimethoxysilane was obtained, which was recorded as Al2O3-CTS-KH560;
[0070] (2) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0071] (3) 14 g and 6 g of BN-CTS-KH560 and Al2O3-CTS-KH560 obtained in step (1) were respectively placed in a container, and 20 g of the silicone oil mixture obtained in step (2) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration of 3000 ppm) were added, and stirred evenly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 hour to obtain a uniform and fluid slurry;
[0072] (4) placing the slurry obtained in step (3) into a vacuum drying oven, degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa, and injecting into a mold after degassing;
[0073] (5) The slurry and the mold are placed in a forced air dryer and heated at 80° C. for 2 h to solidify the slurry. After cooling to room temperature, the slurry is demolded to obtain a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material.
[0074] In Example 4, the filling mass fractions of BN-CTS-KH560 and Al2O3-CTS-KH560 are 35% and 15%, respectively.
[0075] Example 5
[0076] A method for preparing a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material comprises the following steps:
[0077] (1) 0.5 g chitosan (CTS, viscosity <200 mPa·s) and 25 g flake graphite (FG, particle size 200 mesh) were added to 200 ml ethanol aqueous solution (the volume ratio of ethanol to deionized water was 1:3), and then 2 ml glacial acetic acid was added. The mixture was magnetically stirred at 700 rpm for 2 h at room temperature, and then 0.5 g γ-aminopropyltriethoxysilane (KH550) was added. The mixture was stirred for 2 h. After filtration and washing with anhydrous ethanol, the mixture was transferred to a vacuum drying oven and dried at 100°C and -0.10 MPa for 12 h to obtain flake graphite modified with chitosan and γ-aminopropyltriethoxysilane, which was recorded as FG-CTS-KH550.
[0078] Similarly, silicon nitride (Si3N4, particle size 20-30 μm) was modified using the same method, except that for granular fillers such as silicon nitride, the amount of ethanol aqueous solution used was reduced to 100 ml, and the amount of glacial acetic acid used was reduced to 1 ml. Finally, spherical alumina modified with chitosan and γ-aminopropyltriethoxysilane was obtained, which was recorded as Si3N4-CTS-KH550;
[0079] (2) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0080] (3) 16 g and 4 g of FG-CTS-KH550 and Si3N4-CTS-KH550 obtained in step (1) were respectively placed in a container, and 20 g of the silicone oil mixture obtained in step (2) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration of 3000 ppm) were added, and stirred evenly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 hour to obtain a uniform and fluid slurry;
[0081] (4) placing the slurry obtained in step (3) into a vacuum drying oven, degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa, and injecting into a mold after degassing;
[0082] (5) The slurry and the mold are placed in a forced air dryer and heated at 80° C. for 2 h to solidify the slurry. After cooling to room temperature, the slurry is demolded to obtain a chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material.
[0083] In Example 5, the filling mass fractions of FG-CTS-KH550 and Si3N4-CTS-KH550 are 40% and 10%, respectively.
[0084] Comparative Example 1
[0085] A method for preparing a chitosan-modified silicone oil-based flexible thermally conductive composite material comprises the following steps:
[0086] (1) 0.25 g chitosan (CTS, viscosity <200 mPa·s) and 25 g flake graphite (FG, particle size 200 mesh) were added to 200 ml of ethanol aqueous solution (the volume ratio of ethanol to deionized water was 1:3), and then 2 ml of glacial acetic acid was added. The mixture was magnetically stirred at 700 rpm for 4 h at room temperature. After filtration and washing with anhydrous ethanol, the mixture was transferred to a vacuum drying oven and dried at 100°C and -0.10 MPa for 12 h to obtain flake graphite modified with chitosan, which was recorded as FG-CTS.
[0087] Similarly, spherical alumina (S-Al2O3, particle size 50 μm) was modified using the same method, except that for granular fillers such as spherical alumina, the amount of ethanol aqueous solution used was reduced to 100 ml, and the amount of glacial acetic acid used was reduced to 1 ml, and finally spherical alumina modified with chitosan was obtained, which was recorded as Al2O3-CTS;
[0088] (2) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0089] (3) 12 g and 8 g of the FG-CTS and Al2O3-CTS obtained in step (1) were respectively placed in a container, and 20 g of the silicone oil mixture obtained in step (2) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration of 3000 ppm) were added, and stirred evenly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 h to obtain a uniform and fluid slurry;
[0090] (4) placing the slurry obtained in step (3) into a vacuum drying oven, degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa, and injecting into a mold after degassing;
[0091] (5) The slurry and the mold are placed in a blower dryer and heated at 80°C for 2 h to solidify the slurry. After cooling to room temperature, the slurry is demolded to obtain a chitosan-modified silicone oil-based flexible thermal conductive composite material.
[0092] In Comparative Example 1, the filling mass fractions of FG-CTS and Al2O3-CTS are 30% and 20%, respectively.
[0093] Comparative Example 2
[0094] A method for preparing a silane coupling agent-modified silicone oil-based flexible thermally conductive composite material comprises the following steps:
[0095] (1) 25 g of flake graphite (FG, particle size 200 mesh) was added to 200 ml of ethanol aqueous solution (the volume ratio of ethanol to deionized water was 1:3), and then 2 ml of glacial acetic acid and 0.5 g of γ-methacryloxypropyltrimethoxysilane (KH570) were added, and magnetic stirring was performed at 700 rpm at room temperature for 2 h. After filtration and washing with anhydrous ethanol, the mixture was transferred to a vacuum drying oven and dried at 100°C and -0.10 MPa for 12 h to obtain flake graphite modified with γ-methacryloxypropyltrimethoxysilane, which was recorded as FG-KH570;
[0096] Similarly, spherical alumina (S-Al2O3, particle size 50 μm) was modified using the same method, except that for granular fillers such as spherical alumina, the amount of ethanol aqueous solution used was reduced to 100 ml, and the amount of glacial acetic acid used was reduced to 1 ml, and finally spherical alumina modified with γ-methacryloxypropyltrimethoxysilane was obtained, which was recorded as Al2O3-KH570;
[0097] (2) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0098] (3) 12 g and 8 g of FG-KH570 and Al2O3-KH570 obtained in step (1) were respectively placed in a container, and 20 g of the silicone oil mixture obtained in step (2) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration of 3000 ppm) were added, and stirred evenly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 hour to obtain a uniform and fluid slurry;
[0099] (4) placing the slurry obtained in step (3) into a vacuum drying oven, degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa, and injecting into a mold after degassing;
[0100] (5) The slurry and the mold are placed in a blast dryer, heated at 80°C for 2 hours to solidify the slurry, and then demolded after cooling to room temperature to obtain a silane coupling agent-modified silicone oil-based flexible thermal conductive composite material. In Comparative Example 2, the filling mass fractions of FG-KH570 and Al2O3-KH570 are 30% and 20%, respectively.
[0101] Comparative Example 3
[0102] A method for preparing a silicone oil-based flexible thermally conductive composite material comprises the following steps:
[0103] (1) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0104] (2) 12 g of flake graphite (FG, particle size 200 mesh), 8 g of spherical alumina (S-Al2O3, particle size 50 μm), 20 g of the silicone oil mixture obtained in step (1) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration of 3000 ppm) were stirred uniformly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 h to obtain a uniform and fluid slurry;
[0105] (3) placing the slurry obtained in step (2) into a vacuum drying oven and degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa; after degassing, injecting into a mold;
[0106] (4) The slurry and the mold are placed in a blast dryer, heated at 80°C for 2 hours to solidify the slurry, and then demolded after cooling to room temperature to obtain a silicone oil-based flexible thermal conductive composite material. In Comparative Example 3, the filling mass fractions of FG and S-Al2O3 are 30% and 20% respectively.
[0107] Comparative Example 4
[0108] A method for preparing a silicone oil-based flexible thermally conductive composite material comprises the following steps:
[0109] (1) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0110] (2) 14 g of hexagonal boron nitride (h-BN, particle size 20-30 μm), 6 g of spherical alumina (S-Al2O3, particle size 50 μm), 20 g of the silicone oil mixture obtained in step (1) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration 3000 ppm) were stirred uniformly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 h to obtain a uniform and fluid slurry;
[0111] (3) placing the slurry obtained in step (2) into a vacuum drying oven and degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa; after degassing, injecting into a mold;
[0112] (4) The slurry and the mold are placed in a blast dryer, heated at 80°C for 2 hours to solidify the slurry, and then demolded after cooling to room temperature to obtain a silicone oil-based flexible thermal conductive composite material. The filling mass fractions of h-BN and S-Al2O3 in Comparative Example 4 are 35% and 15% respectively.
[0113] Comparative Example 5
[0114] A method for preparing a silicone oil-based flexible thermally conductive composite material comprises the following steps:
[0115] (1) 180.00 g of vinyl-terminated silicone oil (viscosity of 100 mPa·s, vinyl content of 0.98 wt%), 42.15 g of hydrogen-containing silicone oil (hydrogen content of 0.18 wt%), and 0.89 g of ethynyl cyclohexanol (purity of 98%) were placed in a container and magnetically stirred at 500 rpm for 2 h at room temperature to obtain a silicone oil mixture;
[0116] (2) 16 g of flake graphite (FG, particle size 200 mesh), 4 g of silicon nitride (Si3N4, particle size 20-30 μm), 20 g of the silicone oil mixture obtained in step (1) and 50 μL of Karstedt platinum catalyst (zero-valent platinum concentration 3000 ppm) were stirred uniformly with a high-speed stirrer at room temperature at a speed of 800 rpm for 1 h to obtain a uniform and fluid slurry;
[0117] (3) placing the slurry obtained in step (2) into a vacuum drying oven and degassing for 0.5 h at room temperature and a vacuum degree of -0.10 MPa; after degassing, injecting into a mold;
[0118] (4) The slurry and the mold are placed in a blast dryer, heated at 80°C for 2 hours to solidify the slurry, and then demolded after cooling to room temperature to obtain a silicone oil-based flexible thermal conductive composite material. In Comparative Example 5, the filling mass fractions of FG and Si3N4 are 40% and 10% respectively.
[0119] In order to verify the performance of the product of the present invention, the following tests were performed:
[0120] (I) Thermal conductivity test
[0121] The thermal conductivity of the chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite materials of Examples 1-5 and Comparative Examples 1-5 was tested using a Hot-Disk thermal conductivity tester (TPS-2500S).
[0122] (ii) Hardness test
[0123] The hardness of the chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite materials of Examples 1-5 and Comparative Examples 1-5 was tested using a digital display Shore A hardness tester.
[0124] The test results are shown in Table 1 below.
[0125] Table 1
[0126]
[0127] It can be seen from the test results in Table 1 that the thermal conductivity and Shore hardness of Examples 1-5 are better than those of Comparative Examples 1-5, and are greatly improved. The thermal conductivity of Example 1 can reach 1.309 W·m -1 ·K -1, the Shore hardness is as low as 34.5, indicating that the silicone oil-based thermally conductive composite material of the present invention has excellent thermal conductivity and flexibility. The main reason for the improvement of the thermal conductivity of the silicone oil-based flexible thermally conductive composite material modified by chitosan and silane coupling agent is that the silane coupling agent grafted on the surface of the filler improves the compatibility of the filler in the silicone oil matrix, thereby reducing the interfacial thermal resistance between the filler and the matrix. In addition, the chitosan attached to the surface of the filler increases the compatibility of the filler in the matrix, while increasing the hydroxyl groups on the surface of the filler, which is more conducive to the grafting of the silane coupling agent on the surface of the filler, thereby further improving the thermal conductivity of the composite material. The main reason for the decrease in the hardness of the silicone oil-based flexible thermally conductive composite material modified by chitosan and silane coupling agent is that the chitosan attached to the surface of the filler inhibits the silylation reaction of the vinyl-terminated silicone oil and the hydrogen-containing silicone oil, reducing the crosslinking between the two monomers.
[0128] From the comparison of the test results of Example 1 with Comparative Examples 1 and 2, it can be seen that, relative to a single chitosan-modified or silane coupling agent-modified filler, the hardness of the composite material prepared by the chitosan and silane coupling agent-modified filler decreases more significantly, reaching 37%, and its thermal conductivity increases more significantly, reaching 10.7%, indicating that the addition of chitosan and silane coupling agent in the filler modification process has a good synergistic effect on improving the thermal conductivity and reducing the Shore hardness of the silicone oil-based flexible thermally conductive composite material modified by chitosan and silane coupling agent.
[0129] The Chinese invention patent CN101812233A discloses a two-component addition room temperature curing silicone rubber, which uses allyl silicone oil and hydrogen silicone oil as the matrix, and aluminum oxide and quartz powder as thermal conductive fillers, with a thermal conductivity of only 0.7-1.0 W·m -1 ·K -1 The hardness shoreA reaches 45-64, and its performance is far inferior to the chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material of the present invention.
[0130] By comparing the test results of Examples 1-5 with Comparative Examples 1-5, it can be seen that the addition of chitosan and silane coupling agent in the thermal conductive filler modification process proposed by the present invention effectively reduces the hardness of the silicone oil-based flexible thermal conductive composite material modified by chitosan and silane coupling agent, and improves the thermal conductivity of the material, effectively solving the problem that it is difficult to balance high thermal conductivity and low hardness of the thermal conductive composite material. This proves that the silicone oil-based flexible thermal conductive composite material modified by chitosan and silane coupling agent prepared by the present invention has good softness and high thermal conductivity, and can well solve the heat dissipation problem of electronic components.
Claims
1. Silicone oil-based flexible thermal conductive composite material modified by chitosan and silane coupling agent, It is characterized in that The fluid slurry is obtained by heating and solidifying; the fluid slurry is obtained by uniformly stirring a modified flaky filler and a modified granular filler, a silicone oil mixture and a platinum catalyst and then removing bubbles; the modified flaky filler or modified granular filler is obtained by adding chitosan, granular filler or flaky filler to an ethanol aqueous solution, adding glacial acetic acid, stirring uniformly, adding a silane coupling agent and stirring, and filtering, washing and drying after the reaction is completed; In terms of mass percentage, the silicone oil mixture accounts for 50-70% of the raw material mass, the modified flake filler and the modified granular filler account for 30-50% of the raw material mass, of which the flake filler accounts for 20-40% and the granular filler accounts for 10-20%; the silicone oil mixture is obtained by uniformly stirring the vinyl-terminated silicone oil, the side hydrogen-containing silicone oil and the inhibitor; the mass ratio of the vinyl-terminated silicone oil to the side hydrogen-containing silicone oil is 4:1-5:1; the inhibitor is 0.1-1% of the mass of the mixture of the vinyl silicone oil and the side hydrogen-containing silicone oil; the amount of platinum catalyst is not included in the total mass percentage of the raw materials, and 20-30 μL of platinum catalyst is added to every 10 g of the mixture of the vinyl-terminated silicone oil, the side hydrogen-containing silicone oil and the inhibitor; the amount of the silane coupling agent used is 1-2% of the mass of the granular filler and the flake filler; The granular filler is one or more of spherical aluminum oxide, spherical magnesium oxide, aluminum nitride, silicon nitride and silicon carbide; the flaky filler is one or more of flake graphite, hexagonal boron nitride, graphene oxide and graphene; The viscosity of the chitosan is less than 200 mPas, and the amount of chitosan used is 1-2% of the mass of the granular filler and the flaky filler.
2. The chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material according to claim 1, It is characterized in that The volume ratio of deionized water to anhydrous ethanol in the ethanol aqueous solution is 3:1-5:1, the amount of glacial acetic acid used is 1-2 ml added to every 100 ml of the ethanol aqueous solution, the amount of ethanol aqueous solution used in the modification process of the flaky filler is 200-300 ml of ethanol aqueous solution added to every 25 g of the filler; the amount of ethanol aqueous solution used in the modification process of the granular filler is 100-150 ml of ethanol aqueous solution added to every 25 g of the filler.
3. The chitosan and silane coupling agent modified silicone oil-based flexible thermal conductive composite material according to claim 1, It is characterized in that The silane coupling agent is composed of one or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane and vinyltriethoxysilane.
4. The chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material according to claim 3, It is characterized in that The reaction time after adding the silane coupling agent is 1 to 3 hours, and the reaction temperature is room temperature.
5. The chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material according to claim 1, It is characterized in that The vinyl-terminated silicone oil is a divinyl-terminated polydimethylsiloxane with a viscosity of 100-500 mPas and a vinyl content of 0.30-1.10 wt %; the side hydrogen-containing silicone oil is a polymethyl hydrogen siloxane with a hydrogen content of 0.1-0.8 wt %.
6. The chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material according to claim 1, It is characterized in that The inhibitor is ethynyl cyclohexanol, and the catalyst is a Karstedt platinum catalyst, which is a complex formed by zero-valent platinum and divinyltetramethyldisiloxane, and the concentration of zero-valent platinum in the catalyst is 1000-5000 ppm.
7. A method for preparing the chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material according to any one of claims 1 to 6, Features The following steps are involved: (1) adding the chitosan, granular filler or flake filler to an ethanol aqueous solution, adding glacial acetic acid, stirring evenly, adding a silane coupling agent and stirring after the mixture is evenly mixed, and after the reaction is completed, filtering, washing with deionized water and vacuum drying to obtain a modified flake filler or a modified granular filler; (2) Stirring the vinyl-terminated silicone oil, the hydrogen-containing silicone oil and the inhibitor to obtain a silicone oil mixture; (3) adding the modified flaky filler and the modified granular filler obtained in step (1), the silicone oil mixture obtained in step (2), and the platinum catalyst into a container, stirring evenly to obtain a fluid slurry; (4) degassing the fluid slurry and injecting it into a mold; (5) heating and curing the formed product, and demolding the product after cooling to room temperature to obtain a silicone oil-based flexible thermally conductive composite material modified with chitosan and silane coupling agent.
8. The method for preparing the chitosan and silane coupling agent modified silicone oil-based flexible thermally conductive composite material according to claim 7, Features: In step (1), the stirring conditions before and after adding the silane coupling agent are all at a speed of 500-800 rpm, a temperature of room temperature, and a stirring time of 1-2 h; the vacuum drying temperature is 80-100° C., the vacuum degree is -0.08 to -0.10 MPa, and the vacuum drying time is 12-24 h; In step (2), the stirring is performed at room temperature, the stirring speed is 400-600 rpm, and the stirring time is 2-6 hours; In step (3), the stirring is performed at room temperature, the stirring speed is 600-1000 rpm, and the stirring time is 0.5-2 h; In step (4), the degassing is performed by placing the fluid slurry in a vacuum drying oven for vacuum degassing; the vacuum degassing is performed at room temperature and a vacuum degree of -0.10 MPa for 0.5 to 1 hour; In step (5), the heating and curing molding is to place the slurry together with the mold in a blast dryer for heating to solidify the material; the heating temperature of the blast dryer is 60~80℃, and the heating time is 1~2h.