Synergistically strengthened high temperature and high strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening and its preparation method and application
By using a coordinated strengthening of high-temperature high-strength molybdenum alloy with solid solution, dispersion and fine crystal strengthening in high-temperature isothermal forging mold materials, the problems of poor toughness and insufficient oxidation resistance of existing materials at high temperatures are solved, and the high-temperature mechanical properties are achieved. The improvement and simplification of the preparation process meet the needs of high-temperature isothermal forging processes.
Patent Information
- Application Number
- CN202211719719.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The existing high-temperature isothermal forging mold materials have problems such as poor strength and toughness, insufficient oxidation resistance and high toughness and brittle transformation temperature at the operating temperature of 1200°C or above, which is difficult to meet the needs of high-temperature isothermal forging processes. In addition, the existing molybdenum-titanium -Zrconium-carbon alloys are prone to oxidation at high temperatures and have high operating costs.
The coordinated reinforced high-temperature and high-strength molybdenum alloy is adopted, which is composed of Ti, Zr, B, C, La2O3 and other elements, and is prepared by powder metallurgy to form a molybdenum matrix, carbide and oxide structure. Combined with ball milling and cold isostatic pressing processes, the high-temperature mechanical properties and oxidation resistance of the alloy are improved.
It significantly improves the high-temperature and toughness properties of molybdenum alloy, extends its service life, reduces the tough-brittle transition temperature, increases the starting temperature of recrystallization, meets the requirements of high-temperature isothermal forging molds of 1200°C and above, and simplifies preparation The process reduces energy consumption.
Smart Images

Figure CN116219246B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation and application of rare metal structural materials, and in particular relates to a synergistically strengthened high-temperature high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening, and a preparation method and application thereof. Background Art
[0002] With the vigorous development of my country's aviation, aerospace, navigation, military and other national defense industries, higher requirements are placed on the demand for difficult-to-deform materials and high-temperature performance. High-temperature isothermal forging is one of the most important processes for near-net forming of high-temperature difficult-to-deform materials such as powder high-temperature metallurgy. Die materials are the key to the entire high-temperature isothermal forging process of high-temperature alloy materials. Therefore, seeking and developing high-temperature die materials suitable for high-temperature isothermal forging will gradually become a research hotspot and focus.
[0003] Among the existing high temperature isothermal forging die materials, iron-based, nickel-based and other high temperature alloys are currently the most widely used high temperature alloy materials between 650 and 1200°C, and the use temperature is difficult to exceed 1200°C. Therefore, it is urgent to develop high temperature alloys with a use temperature above 1200°C or even higher to meet the growing demand for high temperature isothermal forging die materials.
[0004] At present, high-temperature alloy materials with a use temperature of 1200°C and above are mainly concentrated in refractory / precious metal-based alloy materials such as molybdenum-based, tungsten-based, tantalum-based, niobium-based and platinum-based alloy materials. However, due to the poor room temperature strength and toughness of tungsten alloys, the scarce resources of tantalum, niobium and platinum-based metals are expensive, and they are not suitable for large-scale isothermal forging die materials. Molybdenum alloys have high melting points, good thermal conductivity, low expansion coefficient, slow softening at high temperatures, excellent high and low temperature strength and hardness, high temperature creep, high temperature toughness, and abundant reserves on the earth and are relatively cheap, making them the first choice for high-temperature die materials at 1200°C and above.
[0005] The main micro-strengthening methods of molybdenum alloys are solid solution strengthening (alloying), second phase particle strengthening (dispersion strengthening) and fine grain strengthening. Adding non-metallic or metallic elements (B, C, Si, K, Al, W, Re, Ti, Zr, Hf, etc.) to molybdenum can form solid solution strengthened molybdenum alloys, dispersion strengthened molybdenum alloys or fine grain strengthened molybdenum alloys. However, relying on the strengthening effect of a single strengthening method, the comprehensive performance of molybdenum alloys at high temperature and room temperature is limited, and it is difficult to meet the working requirements of the mold in the high temperature isothermal forging process. For example, adding carbide particles such as TiC, ZrC, TaC, and HfC to molybdenum to obtain a second phase particle strengthened molybdenum alloy, although it has limitedly improved the recrystallization temperature of molybdenum and high temperature properties such as high temperature strength and hardness, but it has limited improvement on the room temperature toughness, oxidation resistance and tough-brittle transition temperature of molybdenum alloys. After working in a high temperature environment, molybdenum alloys are prone to cracking and oxidation, which greatly affects their service life and the working reliability of related structural parts. At present, the most widely used molybdenum-titanium-zirconium-carbon alloy (TZM) for high-temperature molds at 1200°C and above in my country and developed countries such as Europe and the United States, but this alloy is extremely easy to oxidize above 500°C, so it must be used under the protection of vacuum or inert atmosphere. It is necessary to build a dedicated fully enclosed isothermal forging press, which has extremely high operating and maintenance costs. In addition, the frequency of replacement of TZM alloy mold materials is high, and it is necessary to further adjust the composition design of the molybdenum alloy and optimize its additive types and strengthening methods.
[0006] So far, there has been no research on adding different elements to prepare a synergistically strengthened high-temperature and high-strength molybdenum alloy through three strengthening methods: solid solution strengthening, dispersion strengthening and fine grain strengthening to meet the use of high-temperature isothermal forging die materials at 1200°C and above. Summary of the invention
[0007] In view of the scarcity and market demand of high-temperature isothermal forging die materials at 1200°C and above, the present invention provides a synergistically strengthened high-temperature high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening, and a preparation method and application thereof, which specifically include the following contents:
[0008] The first part of the present invention provides a synergistically strengthened high-temperature and high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening. The constituent elements and their mass percentages of the molybdenum alloy are: Ti: 0.4~0.6 wt.%, Zr: 0.15~0.2 wt.%, B: 0.01~0.03 wt.%, C: 0.03~0.05 wt.%, La2O3: 1~1.5 wt.%, the remainder is Mo and unavoidable impurities, and the mass percentages of some constituent elements satisfy the following relationship: Ti+Zr+B+C≤1 wt.%.
[0009] As a further illustration of the present invention, the molybdenum alloy in the sintered state includes a molybdenum matrix, carbides, oxides and a molybdenum alloy.
[0010] As a further illustration of the present invention, the molybdenum alloy is prepared by a powder metallurgy method.
[0011] The second part of the present invention provides the application of the synergistically strengthened high-temperature high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening as described in any of the above items in high-temperature vacuum isothermal forging die materials at 1200°C and above.
[0012] The third part of the present invention provides a method for preparing a synergistically strengthened high temperature and high strength molybdenum alloy by solid solution, dispersion and fine grain strengthening, comprising the following steps:
[0013] (1) vacuum drying molybdenum powder, carbon powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder;
[0014] (2) mixing the vacuum-dried molybdenum powder, carbon powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder according to the mass percentage of the constituent elements of the above-mentioned molybdenum alloy to obtain a premixed powder;
[0015] (3) ball-milling the premixed powder, fully mixing and sieving to make the powder particle size ≤5 μm to obtain a mixed alloy powder;
[0016] (4) pressing the mixed alloy powder into a cylindrical green body under a cold isostatic press at 200-250 MPa for 10-15 min;
[0017] (5) placing the cylindrical green body in a hydrogen sintering furnace and sintering it under a hydrogen atmosphere;
[0018] (6) After sintering, the alloy billet is cooled to room temperature in a hydrogen atmosphere and then taken out to obtain a molybdenum alloy billet.
[0019] As a further illustration of the present invention, the purity of the raw materials in step (1) is: Mo ≥ 99.97%, TiH2 ≥ 99.97%, of which Ti ≥ 99.59%, Zr+Hf+H in ZrH2 ≥ 99.97%, of which Zr+Hf ≥ 97.6%; boron powder and graphite powder are both analytically pure, and the conditions for vacuum drying are: temperature: 100°C; vacuum degree: -0.1 MPa; drying time: 4 h.
[0020] As a further illustration of the present invention, in step (3), a planetary ball mill is used for ball milling, the ball milling time is 2 h, the rotation speed is 240 r / min, and the ball-to-material ratio is 2:1.
[0021] As a further illustration of the present invention, the diameter of the cylindrical green body formed by cold isostatic pressing in the step (4) is 40 mm, and the hydrogen in the step (4) is high-purity hydrogen.
[0022] As a further illustration of the present invention, the sintering process in step (5) is specifically as follows: firstly, the temperature is gradually increased from room temperature to 200°C and then kept at this temperature to fully remove free water in the mixed powder; then, the temperature is quickly increased to 900°C and kept at this temperature to remove volatile impurities in the mixed powder and reduce the reaction between Mo and O in the powder; after the 900°C is kept at this temperature, the temperature is slowly increased to 1200°C and kept at this temperature to further remove some impurities; then, the temperature is slowly increased to 1900°C and sintered at high temperature for 4 h to promote the formation of the alloy, and after the high temperature sintering is completed, the alloy rod is cooled in the furnace to obtain a sintered alloy rod. The specific sintering process is as follows: Figure 1 shown.
[0023] As a further illustration of the present invention, the relative density of the molybdenum alloy after high temperature sintering in step (6) is greater than 98%.
[0024] Compared with the prior art, the present invention has the following beneficial technical effects:
[0025] 1. The high-strength and high-temperature molybdenum alloy designed and prepared by the present invention is composed of a molybdenum matrix, carbides, oxides and molybdenum alloys, and has a recrystallization start temperature of ≥1400°C, and has excellent comprehensive mechanical properties of yield strength ≥510 MPa, tensile strength ≥590 MPa and plastic deformation of about 15% at 1200°C;
[0026] 2. The high-temperature high-strength molybdenum alloy designed and prepared by the present invention, by adding elements such as Ti, Zr, B, and C, the grains are refined by the strong pinning effect of the formed TiC, ZrC, B2C and other carbides on dislocations, resulting in fine grain strengthening; and a small amount of solid solution formed by Ti, Zr, B and their corresponding carbides and molybdenum, resulting in solid solution strengthening, and second phase particles formed by Ti, Zr, B and their corresponding carbides and oxides, resulting in dispersion strengthening, which can significantly improve the high-temperature strength and toughness of the molybdenum alloy, meet the high-temperature working conditions of high-temperature isothermal forging dies at 1200°C and above, and at the same time slow down the generation and expansion of cracks in the alloy under working conditions, greatly improve the room temperature brittleness of the molybdenum alloy, and effectively reduce the toughness-brittleness transition temperature of the molybdenum alloy, while increasing its recrystallization start temperature;
[0027] 3. The high-temperature, high-strength molybdenum alloy designed and prepared by the present invention can refine the molybdenum alloy grains and produce fine grain strengthening by adding rare earth La2O3; and form second phase particles to produce dispersion strengthening, and at the same time can greatly improve the high-temperature mechanical properties and oxidation resistance of the molybdenum alloy. The alloy material is directly processed under the sintered state cooling conditions of sintering into rods, without the need for solid solution and aging processes, and is simple to prepare, low in energy consumption and high in efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1The sintering process diagram of the synergistically strengthened high-temperature and high-strength molybdenum alloy provided by the present invention is provided by solid solution, dispersion and fine grain strengthening. DETAILED DESCRIPTION
[0029] In order to make the technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The alloy structure and performance of the embodiments of the present application shown in the drawings here can be regulated and designed with various different composition configurations. Therefore, the following detailed description of the embodiments of the present application provided in the drawings is not intended to limit the scope of the application claimed for protection, but only represents the selected embodiments of the present application. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0030] The technical solution of the present application will be explained below in conjunction with specific embodiments. Example 1
[0031] Provided is a synergistically strengthened high-temperature high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening, the alloy consists of carbon, zirconium, titanium, lanthanum, oxygen and molybdenum elements; wherein the mass percentage ranges are: Ti: 0.45 wt.%, Zr: 0.18 wt.%, B: 0.02 wt.%, C: 0.04 wt.%, La2O3: 1 wt.%, the remainder being Mo and unavoidable impurities, all of which are mass percentages.
[0032] The preparation method of the above-mentioned synergistically strengthened high-temperature high-strength molybdenum alloy comprises the following steps:
[0033] Step 1: vacuum dry molybdenum powder, carbon powder, boron powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder (raw material purity: Mo ≥ 99.97%, TiH2 ≥ 99.97%, of which Ti ≥ 99.59%, Zr+Hf+H in ZrH2 ≥ 99.97%, of which Zr+Hf ≥ 97.6%, boron powder and graphite powder are both analytical grade); the vacuum drying conditions are: temperature: 100°C; vacuum degree: -0.1MPa; drying time: 4 h.
[0034] Step 2: Mix the vacuum-dried molybdenum powder, carbon powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder according to the above preset composition ratio to obtain a premixed powder;
[0035] Step 3: placing the premixed powder in a planetary ball mill for ball milling, fully mixing and sieving to make the powder particle size ≤ 5 μm to obtain a mixed alloy powder;
[0036] Step 4: cold isostatically press the mixed alloy powder at 250 MPa for 10 min to prepare a cylindrical green body with a diameter of 40 mm;
[0037] Step 5: Place the cylindrical green body in a hydrogen sintering furnace and sinter it in a hydrogen atmosphere according to Figure 1 The sintering process shown is to carry out high temperature hydrogen sintering to prepare molybdenum alloy rod blanks;
[0038] Step 6: After sintering, the alloy billet is cooled to room temperature in a hydrogen atmosphere and then taken out to obtain an alloy billet.
[0039] Step 7: The obtained alloy rod blank is sampled for high temperature mechanical property and hardness test. The yield strength at 1200°C is 515.6 MPa, the tensile strength is 594 MPa, the elongation is 16.3%, and the recrystallization start temperature is greater than 1400°C. Example 2
[0040] Provided is a synergistically strengthened high-temperature high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening, the alloy consists of carbon, zirconium, titanium, lanthanum, oxygen and molybdenum elements; wherein the mass percentage ranges are: Ti: 0.5 wt.%, Zr: 0.18 wt.%, B: 0.02 wt.%, C: 0.04 wt.%, La2O3: 1.2 wt.%, the remainder being Mo and unavoidable impurities, all of which are mass percentages.
[0041] The preparation method of the above-mentioned synergistically strengthened high-temperature high-strength molybdenum alloy comprises the following steps:
[0042] Step 1: vacuum dry molybdenum powder, carbon powder, boron powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder (raw material purity: Mo ≥ 99.97%, TiH2 ≥ 99.97%, of which Ti ≥ 99.59%, Zr+Hf+H in ZrH2 ≥ 99.97%, of which Zr+Hf ≥ 97.6%, boron powder and graphite powder are both analytical grade); the vacuum drying conditions are: temperature: 100°C; vacuum degree: -0.1MPa; drying time: 4 h.
[0043] Step 2: Mix the vacuum-dried molybdenum powder, carbon powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder according to the above preset composition ratio to obtain a premixed powder;
[0044] Step 3: placing the premixed powder in a planetary ball mill for ball milling, fully mixing and sieving to make the powder particle size ≤ 5 μm to obtain a mixed alloy powder;
[0045] Step 4: cold isostatically press the mixed alloy powder at 250 MPa for 15 min to prepare a cylindrical green body with a diameter of 40 mm;
[0046] Step 5: Place the cylindrical green body in a hydrogen sintering furnace and sinter it in a hydrogen atmosphere according to Figure 1 The sintering process shown is to carry out high temperature hydrogen sintering to prepare molybdenum alloy rod blanks;
[0047] Step 6: After sintering, the alloy billet is cooled to room temperature in a hydrogen atmosphere and then taken out to obtain an alloy billet.
[0048] Step 7: The obtained alloy rod blank is sampled for high temperature mechanical property and hardness test. The yield strength at 1200°C is 565.8 MPa, the tensile strength is 643.4 MPa, the elongation is 21.5%, and the recrystallization start temperature is greater than 1400°C. Example 3
[0049] Provided is a synergistically strengthened high-temperature high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening, the alloy consists of carbon, zirconium, titanium, lanthanum, oxygen and molybdenum elements; wherein the mass percentage ranges are: Ti: 0.6 wt.%, Zr: 0.2 wt.%, B: 0.3 wt.%, C: 0.05 wt.%, La2O3: 1.5 wt.%, the remainder being Mo and unavoidable impurities, all of which are mass percentages.
[0050] The preparation method of the above-mentioned synergistically strengthened high-temperature high-strength molybdenum alloy comprises the following steps:
[0051] Step 1: vacuum dry molybdenum powder, carbon powder, boron powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder (raw material purity: Mo ≥ 99.97%, TiH2 ≥ 99.97%, of which Ti ≥ 99.59%, Zr+Hf+H in ZrH2 ≥ 99.97%, of which Zr+Hf ≥ 97.6%, boron powder and graphite powder are both analytical grade); the vacuum drying conditions are: temperature: 100°C; vacuum degree: -0.1MPa; drying time: 4 h.
[0052] Step 2: Mix the vacuum-dried molybdenum powder, carbon powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder according to the above preset composition ratio to obtain a premixed powder;
[0053] Step 3: placing the premixed powder in a planetary ball mill for ball milling, fully mixing and sieving to make the powder particle size ≤ 5 μm to obtain a mixed alloy powder;
[0054] Step 4: cold isostatically press the mixed alloy powder at 250 MPa for 15 min to prepare a cylindrical green body with a diameter of 40 mm;
[0055] Step 5: Place the cylindrical green body in a hydrogen sintering furnace and sinter it in a hydrogen atmosphere according to Figure 1The sintering process shown is to carry out high temperature hydrogen sintering to prepare molybdenum alloy rod blanks;
[0056] Step 6: After sintering, the alloy billet is cooled to room temperature in a hydrogen atmosphere and then taken out to obtain an alloy billet.
[0057] Step 7: The obtained alloy rod blank is sampled for high temperature mechanical property and hardness test. The yield strength at 1200°C is 588 MPa, the tensile strength is 677.4 MPa, the elongation is 25.7%, and the recrystallization start temperature is greater than 1400°C.
[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A synergistically strengthened high temperature and high strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening, characterized in that: The molybdenum alloy has the following constituent elements and their mass percentages: Ti: 0.4-0.6 wt.%, Zr: 0.15-0.2 wt.%, B: 0.01-0.03 wt.%, C: 0.03-0.05 wt.%, La2O3: 1-1.5 wt.%, and the remainder is Mo and unavoidable impurities; The high-temperature and high-strength molybdenum alloy synergistically strengthened by solid solution, dispersion and fine grain strengthening can be used in high-temperature vacuum isothermal forging die materials at 1200°C and above, and the high-temperature and high-strength molybdenum alloy synergistically strengthened by solid solution, dispersion and fine grain strengthening has a yield strength of ≥510 MPa, a tensile strength of ≥590 MPa and a plastic deformation of 15% at 1200°C.
2. The synergistically strengthened high temperature and high strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening according to claim 1, characterized in that: The molybdenum alloy comprises a molybdenum matrix, carbides, oxides and a molybdenum alloy in a sintered state.
3. The synergistically strengthened high temperature and high strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening according to claim 1, characterized in that: The molybdenum alloy is prepared by a powder metallurgy method.
4. A method for preparing a high-temperature high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening, characterized in that: The following steps are involved: (1) vacuum drying molybdenum powder, carbon powder, boron powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder; (2) mixing the vacuum-dried molybdenum powder, carbon powder, boron powder, zirconium hydride powder, titanium hydride powder and rare earth lanthanum oxide powder according to the mass percentage of the constituent elements of the molybdenum alloy according to claim 1 to obtain a premixed powder; (3) ball-milling the premixed powder, fully mixing and sieving to make the powder particle size ≤5 μm to obtain a mixed alloy powder; (4) Pressing the mixed alloy powder into a cylindrical green body under a cold isostatic press at 200-250 MPa for 10-15 min; (5) placing the cylindrical green body in a hydrogen sintering furnace and sintering it under a hydrogen atmosphere; (6) After sintering, the alloy billet is cooled to room temperature in a hydrogen atmosphere and taken out to obtain a molybdenum alloy billet having a yield strength of ≥510 MPa, a tensile strength of ≥590 MPa and a plastic deformation of 15% at 1200°C.
5. The method for preparing a synergistically strengthened high temperature and high strength molybdenum alloy by solid solution, dispersion and fine grain strengthening according to claim 4, characterized in that: The purity of the raw materials in step (1) is: Mo ≥ 99.97%, TiH2 ≥ 99.97%, of which Ti ≥ 99.59%, Zr+Hf+H in ZrH2 ≥ 99.97%, of which Zr+Hf ≥ 97.6%; the conditions for the vacuum drying are: temperature: 100°C; Vacuum degree: -0.1 MPa; Drying time: 4 h.
6. The method for preparing a high-temperature and high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening according to claim 4, characterized in that: In the step (3), a planetary ball mill is used for ball milling, the ball milling time is 2 h, the rotation speed is 240 r / min, and the ball-to-material ratio is 2:
1.
7. The method for preparing a high-temperature and high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening according to claim 4, characterized in that: The diameter of the cylindrical green body formed by cold isostatic pressing in the step (4) is 40 mm.
8. The method for preparing a high-temperature and high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening according to claim 4, characterized in that: The sintering process in step (5) is specifically as follows: firstly, the temperature is gradually increased from room temperature to 200°C and then kept at this temperature, then the temperature is quickly increased to 900°C and kept at this temperature, after the temperature is kept at 900°C, the temperature is slowly increased to 1200°C and kept at this temperature, then the temperature is slowly increased to 1900°C and high-temperature sintered for 4 h, and after the high-temperature sintering is completed, the temperature is cooled in the furnace to obtain a sintered alloy rod.
9. The method for preparing a high-temperature and high-strength molybdenum alloy strengthened by solid solution, dispersion and fine grain strengthening according to claim 4, characterized in that: The relative density of the alloy rod obtained after high-temperature sintering of the molybdenum alloy in step (6) is greater than 98%.