A low temperature preparation method of MAX phase coating and its application
The MAX phase coating is deposited under low temperature conditions through DC magnetron sputtering composite double-target high-power pulse magnetron sputtering technology, which solves the problems of high phase formation temperature and impurity phase generation in the existing technology, and achieves high-purity MAX phase coating. The preparation and performance improvement of the coating have expanded its application in high-temperature and harsh corrosive environments.
Patent Information
- Application Number
- CN202211603528.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-13
AI Technical Summary
In the existing preparation methods of MAX phase materials, the phase formation temperature is high, which leads to the generation of impurity phases and the reduction of material properties during the preparation process, limiting its application in high-temperature and harsh corrosive environments.
DC magnetron sputtering composite double target high-power pulse magnetron sputtering technology is used to deposit Ti2AlC, Cr2AlC and V2AlC MAX phase coatings improve the composition control accuracy and kinetic energy of film-forming particles, and reduce the phase formation temperature.
The low-temperature preparation of high-purity (>90wt.%) MAX phase coating is achieved, which reduces the phase formation temperature of traditional PVD technology, improves the oxidation corrosion resistance and surface smoothness of the coating, and expands the application field of the material.
Smart Images

Figure CN116219381B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material surface treatment, and in particular relates to a low-temperature preparation method of a MAX phase coating and application thereof. Background Art
[0002] M n+1 AX n Phase (n = 1, 2 or 3, referred to as MAX phase) is a large class of thermodynamically stable nano-layered metal carbide or nitride ceramic materials with a close-packed hexagonal structure. M mainly represents IVB-VIB pre-transition metals (Ti, Cr, V, etc.), A mainly comes from IIIA or IVA main group elements (Al, Si, etc.), and X represents C or N. Ti2AlC, Cr2AlC, and V2AlC contain Ti, Cr, V, and Al elements at the same time, and have excellent heat corrosion resistance and high-temperature oxidation resistance, and are typical representatives of MAX phase materials; in addition, the preferential diffusion and oxidation of Al atoms also make MAX phase materials have good self-healing ability; and it also has thermophysical properties that match stainless steel, high-performance Ti alloys and other materials. These excellent properties make Al-based Ti2AlC, Cr2AlC, and V2AlC coatings very suitable for surface protection of materials with complex working conditions such as alternating heat loads, oxidation, and multi-factor coupled corrosion, such as key components of high-performance aircraft engines and gas turbines (collectively referred to as "two engines") in severe marine corrosion environments.
[0003] However, MAX phase materials not only have strict chemical composition, but also have complex unit cell structure and large c-axis unit cell parameters (such as 211 series Cr2AlC c-axis length ), which makes it difficult to prepare high-purity phases, the atomic diffusion distance required for crystallization is long, and the preparation temperature is high. In the common preparation methods of MAX phase bulk materials, such as vacuum pressureless sintering, hot isostatic pressing, arc melting and pulse discharge sintering, the synthesis temperature is above 1100°C, and the synthetic products are often accompanied by TiC, TiAl x ,CrC x or AlCr x Impurity phases such as compounds reduce the protective properties of the material.
[0004] For the 211 series Ti2AlC, Cr2AlC, and V2AlC MAX phase protective coating materials, the current preparation methods are mainly PVD technologies such as magnetron sputtering and cathode arc ion plating, but their phase formation temperatures are often in the range of 450 to 900°C, which is still higher than the performance degradation temperature (~450°C) of commonly used Ti alloys and stainless steel materials, limiting their surface protection applications in key areas of major technical equipment.
[0005] In summary, since MAX phase materials have many competing phases, complex structures, and high phase formation temperatures, how to lower the preparation temperature of MAX phase coatings and achieve high-purity and low-temperature crystallization of MAX phase coatings is one of the bottlenecks that urgently need to be broken through in order to expand the application fields of MAX phase materials. This has important research value and significance for expanding the application fields of this material, especially for its application in high-temperature and harsh corrosive environments in the ocean. Summary of the invention
[0006] The main purpose of the present invention is to provide a low-temperature preparation method of a MAX phase coating and its application to overcome the shortcomings of the prior art.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0008] An embodiment of the present invention provides a low-temperature preparation method of a MAX phase coating, which comprises:
[0009] providing a substrate;
[0010] and, using a DC magnetron sputtering composite dual-target high power pulse magnetron sputtering technology (Hybrid Direct Current Magnetron Sputtering and Dual-magnetron High Power Impulse Magnetron Sputtering, Hybrid DCMS / DM-HiPIMS) to deposit a MAX phase coating on the surface of the substrate;
[0011] Among them, the target material used in the DC magnetron sputtering technology is an Al target, and the dual-target target materials used in the dual-target high-power pulsed magnetron sputtering technology are a metal target and a C target, respectively. The metal target is selected from a Ti target, a Cr target or a V target, and the magnetic field between any two targets among the metal target, the C target and the Al target is a closed magnetic field with opposite magnet polarities or a mirror magnetic field with the same magnet polarity; the deposition temperature is 350-500°C.
[0012] An embodiment of the present invention further provides a MAX phase coating prepared by the aforementioned low-temperature preparation method, wherein the atomic ratio in the MAX phase coating is 2:1:1, and the MAX phase coating includes any one of Ti2AlC, Cr2AlC, and V2AlC.
[0013] The embodiment of the present invention also provides the use of the MAX phase coating prepared by the aforementioned low-temperature preparation method in the field of protection in the high-temperature and severe corrosive environment of the ocean.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] (1) The present invention uses a DC power supply to sputter an Al target, and a composite high-power pulse power supply to sputter a Ti / Cr / V target and a C target. The DC discharge of the Al target plays a role in pre-ionizing the background gas, which can improve the stability and continuity of HiPIMS discharge at low pressure and reduce the loss of sputtered particle energy during transmission. At the same time, the lower duty cycle and higher peak power density in the high-power discharge of the Ti / Cr / V target and the C target not only improve the accuracy of the control of the composition of the film-forming particles, but also enhance the kinetic energy of the particles incident on the substrate surface and extend the diffusion distance of the film-forming particles, so that a high-purity MAX phase coating can be prepared at a lower substrate heating temperature, reducing the phase formation temperature required for preparing the MAX phase by PVD technology. The present invention prepares a high-purity (>90wt.%) MAX phase coating at 350-500°C (conventional 450-900°C), providing a new idea for the preparation of MAX phase coatings.
[0016] (2) The dual-target high-power pulsed magnetron sputtering technology in the present invention combines the advantages of traditional magnetron sputtering, such as low-temperature deposition, uniform and smooth surface, and no large particle defects, and arc ion plating, such as high cathode material ionization rate, strong film-substrate bonding, and dense coating. At the same time, it improves the problems of low target material utilization and narrow sputtering zone existing in traditional magnetron sputtering, so that the surface of the prepared coating has no large particle accumulation phenomenon, and the coating surface is smooth, uniform in composition, dense in structure, and the roughness is as low as 10-50nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 This is a discharge characteristic diagram of a DC magnetron sputtering composite dual-target high-power pulsed magnetron sputtering power supply in preparing a Cr2AlC MAX phase coating in Example 1 of the present invention;
[0019] Figure 2 1 is the XRD spectra of the MAX phase coatings prepared in Example 1 of the present invention and Comparative Example 1;
[0020] Figure 3 1 is a Raman spectrum of the MAX phase coating prepared in Example 1 of the present invention and Comparative Example 1;
[0021] Figure 4 is a surface morphology image of the MAX phase coating prepared in Example 1 of the present invention;
[0022] Figure 5is a surface morphology of the MAX phase coating prepared in Comparative Example 1 of the present invention;
[0023] Figure 6 1 is the XRD spectra of the MAX phase coatings prepared in Example 2 of the present invention and Comparative Example 2;
[0024] Figure 7 1 is a Raman spectrum of the MAX phase coating prepared in Example 2 of the present invention and Comparative Example 2;
[0025] Figure 8 is a surface morphology image of the MAX phase coating prepared in Example 2 of the present invention;
[0026] Fig. 9 It is a surface morphology picture of the MAX phase coating prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0027] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The present invention is designed to use composite DC magnetron sputtering and composite dual-target high-power pulsed magnetron sputtering technology to achieve high-purity low-temperature preparation of MAX phase coatings. The DCMS pre-ionization background gas is used to improve the stability and continuity of HiPIMS discharge at low pressure and reduce the energy loss in the deposition process of target sputtering particles; at the same time, the closed magnetic field DC pre-ionization can effectively enhance the ionization rate of film-forming atoms in HiPIMS discharge, which is conducive to the use of bias voltage to accurately control the particle composition and kinetic energy, so that the Ti / Cr / V, Al and C atoms incident on the substrate surface can obtain sufficient diffusion capacity to form a crystalline MAX phase coating; and a higher ionization rate of film-forming particles can enhance the coupling efficiency of the pulse bias voltage, which is conducive to the formation of a dense coating structure and further improves the oxidation corrosion resistance of the coating.
[0028] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Specifically, as one aspect of the technical solution of the present invention, a low-temperature preparation method of a MAX phase coating involves:
[0030] providing a substrate;
[0031] And, using DC magnetron sputtering composite dual-target high-power pulsed magnetron sputtering technology to deposit and form a MAX phase coating on the surface of the substrate;
[0032] Among them, the target material used in the DC magnetron sputtering technology is an Al target, and the dual-target target materials used in the dual-target high-power pulsed magnetron sputtering technology are a metal target and a C target, respectively. The metal target is selected from a Ti target, a Cr target or a V target, and the magnetic field between any two targets among the metal target, the C target and the Al target is a closed magnetic field with opposite magnet polarities or a mirror magnetic field with the same magnet polarity; the deposition temperature is 350-500°C.
[0033] Specifically, the MAX phase coating in the present invention is obtained by sputtering high-purity Ti / Cr / V, Al and C single-substance targets. From the beginning of deposition, the Al target is sputtered by DCMS technology, and the Ti / Cr / V and C targets are sputtered by HiPIMS technology. The parameters of the HiPIMS power supply are set as follows: frequency is 100-1000Hz; duty cycle is 2.5-5%; pulse width is 25-500μs. Under a certain substrate preheating temperature, crystalline Ti2AlC, Cr2AlC, V2AlC MAX phase coatings are directly obtained.
[0034] Preferably, in the coating deposition of the present invention, the duty cycle of the Ti / Cr / V target is preferably 2.5%, the pulse width is 50 μs, and the pulse bias amplitude is 0 V, thereby achieving high-purity and low-temperature preparation of Ti2AlC, Cr2AlC, and V2AlC MAX phase coatings.
[0035] In some preferred embodiments, the low-temperature preparation method specifically includes: placing the substrate in a reaction chamber, turning on a DC magnetron sputtering power supply and a high-power pulsed magnetron sputtering power supply, self-cleaning the target for 20 to 30 minutes, and then depositing a MAX phase coating;
[0036] Among them, the power of the Al target in the DC magnetron sputtering is 15-35W, and the power supply parameters of the dual-target high-power pulsed magnetron sputtering technology are set as: frequency is 100-1000Hz, duty cycle is 2.5-5%, pulse width is 25-500μs, the power of the metal target is 50-100W, the power of the C target is 100-200W, and the substrate bias is -200-0V.
[0037] Furthermore, the pulse width is the pulse time.
[0038] In some preferred embodiments, the purity of the target material is above 99.99% and the size is But it is not limited to cylindrical targets and rectangular targets of this size.
[0039] In some preferred embodiments, the working gas used in the formation process of the MAX phase coating includes any one of neon, argon, krypton, and xenon, or a combination of two or more thereof, but is not limited thereto.
[0040] In some preferred embodiments, the low-temperature preparation method further comprises: placing the substrate in a reaction, evacuating the vacuum to 5×10 -4 Pa, the substrate is heated and Ar gas is introduced into the cavity to perform Ar plasma etching and cleaning treatment on the substrate surface.
[0041] Furthermore, during the Ar plasma etching and cleaning process, the Ar gas flow rate is 20-50 sccm, the substrate negative bias frequency is 150-350 kHz, the amplitude is 400-800 V, and the duty cycle is 50-70%.
[0042] In some preferred embodiments, the low-temperature preparation method further comprises: first polishing and ultrasonic cleaning the substrate; preferably, the cleaning liquid used in the ultrasonic cleaning includes acetone and / or ethanol, but is not limited thereto.
[0043] In some preferred embodiments, the matrix includes Ti-6Al-4V, but is not limited thereto.
[0044] In some more specific embodiments, the low temperature preparation method of the MAX phase coating comprises:
[0045] (1) The Ti-6Al-4V alloy sheet is placed in acetone and alcohol for cleaning and drying.
[0046] Preferably, ultrasonic cleaning is used, and the cleaning time is preferably 10 minutes.
[0047] Preferably, after cleaning, the substrate is rinsed with deionized water, then blown dry with high-purity N2 and placed on a rack.
[0048] (2) Place the Ti-6Al-4V alloy sheet in the deposition vacuum chamber and evacuate to 5×10 -4 Pa, heated to 350-500°C, Ar gas was introduced into the vacuum chamber, a pulsed negative bias was applied to the substrate, and the surface of the substrate was cleaned and etched using Ar plasma.
[0049] Preferably, the Ar gas pressure is 2-5 Pa.
[0050] Preferably, the amplitude of the pulse negative bias voltage is 400-800V.
[0051] Preferably, the etching time is 15 to 30 minutes.
[0052] (3) Under the protection of Ar atmosphere, the Al target, Ti target / Cr target / V target and C target power are turned on, and the target material is self-cleaned by magnetron sputtering.
[0053] Preferably, the Ar gas pressure is 0.4-0.8Pa.
[0054] Preferably, the power of the Al target, Ti target / Cr target / V target and C target is 100-200W.
[0055] Preferably, the cleaning time is 15 to 30 minutes.
[0056] (4) When the working gas is Ar gas, a pulsed negative bias voltage is applied to the substrate, the power supplies of the Al target, Ti / Cr / V target and C target are turned on, and the MAX phase coating is deposited on the surface of the substrate by magnetron sputtering.
[0057] Preferably, the working gas pressure is 0.4-0.8Pa.
[0058] Preferably, the amplitude of the pulse negative bias voltage is 0-200V.
[0059] Preferably, the Al target power is 15-35W, the Ti, Cr, and V target power is 50-100W, and the C target power is 100-200W.
[0060] Preferably, the sputtering time is 240 to 1200 minutes.
[0061] Preferably, the substrate rotation speed during sputtering is 5 to 20 revolutions per minute.
[0062] Preferably, in the step (4), the crystallinity of the deposited MAX phase coating is controlled by controlling the HiPIMS power frequency, duty cycle, substrate bias, etc., thereby further reducing the crystallization temperature of the MAX phase coating.
[0063] The preparation method of the MAX phase coating provided by the present invention reduces the deposition temperature by at least 100° C. compared with the traditional method when preparing the same MAX phase coating.
[0064] Another aspect of an embodiment of the present invention further provides a MAX phase coating prepared by the aforementioned low-temperature preparation method, wherein the atomic ratio in the MAX phase coating is 2:1:1, and the MAX phase coating includes any one of Ti2AlC, Cr2AlC, and V2AlC.
[0065] Furthermore, the purity of the MAX phase coating is greater than 90wt%, and the surface roughness is 10-50nm.
[0066] Furthermore, the thickness of the MAX phase coating is 2-10 μm.
[0067] Another aspect of the embodiments of the present invention further provides the use of the MAX phase coating prepared by the aforementioned low-temperature preparation method in the field of protection in high-temperature and severe corrosive environments in the ocean.
[0068] For example, the MAX phase coating prepared by the present invention is applied to the Ti-6Al-4V material of aircraft engine blades.
[0069] The MAX phase coating prepared by the present invention can effectively protect the substrate in a high temperature, high salt, high humidity and high heat environment.
[0070] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0071] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0072] Embodiment 1:
[0073] In this embodiment, the substrate material is a Ti-6Al-4V alloy sheet (TC4 alloy sheet), and the specific preparation steps of the Cr2AlC MAX phase coating on the substrate surface are as follows:
[0074] Step 1: Use 400# to 3000# SiC sandpaper to grind the surface of TC4 alloy sheet in turn, and then use 2.5μm diamond polishing agent to polish for 20 minutes.
[0075] Step 2: Place the polished TC4 alloy sheet substrate in acetone and alcohol for ultrasonic cleaning for 10 minutes, then rinse with deionized water, and then blow dry with high-purity N2, and use a metal press to fix the substrate on the rack for use.
[0076] Step 3: Place the rack in the deposition chamber and wait for the mechanical pump and molecular pump to evacuate to 5×10 -4 Pa and after the substrate heating temperature reaches 350°C, high-purity Ar gas with a pressure of 2.0 Pa is introduced into the vacuum chamber, the pulse negative bias power supply frequency is set to 350 kHz, the amplitude is 600 V, and the duty cycle is 60%, and the TC4 alloy substrate is etched and cleaned for 20 min.
[0077] Step 4: Introduce high-purity Ar gas with a pressure of 0.5 Pa into the vacuum chamber. When the Al target and the Cr / C target both form a closed magnetic field, and the Cr target and the C target form a mirror magnetic field, turn on the DC power supply of the Al target, and turn on the high-power pulse power supply of the Cr target and the C target at the same time, and use magnetron sputtering to self-clean each target material.
[0078] Step 5: High-purity Ar gas with a pressure of 0.5 Pa is introduced into the vacuum chamber. Under the magnetic pole configuration in which the Al target and the Cr / C target both form a closed magnetic field, and the Cr target and the C target form a mirror magnetic field, the Al target DC power supply is turned on with a power of 20 W; at the same time, the high-power pulse sputtering power supplies of the Cr target and the C target are turned on with the powers set to 65 W and 135 W, respectively. The parameters of the HiPIMS power supply are set as follows: frequency, 500 Hz, period 2000 μs, Cr target duty cycle of 2.5%, pulse time 50 μs, C target duty cycle of 5%, pulse time 100 μs, and multi-target magnetron co-sputtering is used to deposit the Cr2AlC MAX phase coating. The substrate bias is 0 V and the deposition time is 240 min. The discharge characteristics during the deposition process are as follows: Figure 1 As shown in the figure, it can be seen that both the Cr target and the C target are at a higher peak power density (350W / cm 2 With 325W / cm 2 ) under the splash.
[0079] Comparative Example 1:
[0080] This embodiment is a comparative embodiment of the above-mentioned embodiment 1.
[0081] In this embodiment, the substrate is exactly the same as in Example 1, and the polishing, cleaning and surface Ar plasma etching cleaning processes of the substrate are also exactly the same. The difference is that in steps 4 and 5, the sputtering of Al, Cr, and C targets all uses a traditional DC power supply instead of a high-power pulse power supply, and the DC sputtering source during the deposition process is also set to a constant power of 20W, 65W, and 135W.
[0082] Figure 2 and Figure 3 The X-ray diffraction spectrum and Raman spectrum of the coating obtained in Example 1 and Comparative Example 1 are as follows. Figure 2 and Figure 3 It can be seen that the deposited coating prepared by DC composite dual-target high-power pulsed magnetron sputtering technology is a crystalline Cr2AlCMAX phase coating, while the deposited coating prepared by multi-target DC magnetron sputtering in Comparative Example 1 is amorphous. There are also some characteristic diffraction peaks from the substrate in the XRD spectrum.
[0083] Figure 4 and Figure 5 They are the surface morphology pictures of the coatings prepared in the above-mentioned Example 1 and Comparative Example 1 respectively. The surface of the deposited coating prepared by the DC composite dual-target high-power pulsed magnetron sputtering technology shows obvious MAX phase layer growth crystallization characteristics, while the surface of the coating prepared by DC magnetron co-sputtering is very smooth, showing obvious amorphous coating characteristics.
[0084] Embodiment 2:
[0085] In this embodiment, the substrate material is a Ti-6Al-4V alloy sheet, and the specific preparation steps of the Cr2AlC MAX phase coating on the substrate surface are as follows:
[0086] Step 1: Use 400# to 3000# SiC sandpaper to grind the surface of TC4 alloy sheet in turn, and then use 2.5μm diamond polishing agent to polish for 20 minutes.
[0087] Step 2: Place the polished TC4 alloy sheet substrate in acetone and alcohol for ultrasonic cleaning for 10 minutes, then rinse with deionized water, and then blow dry with high-purity N2, and use a metal press to fix the substrate on the rack for use.
[0088] Step 3: Place the rack in the deposition chamber and wait for the mechanical pump and molecular pump to evacuate to 5×10 -4 Pa and after the substrate heating temperature reaches 350°C, high-purity Ar gas with a pressure of 2.0 Pa is introduced into the vacuum chamber, the pulse negative bias power supply frequency is set to 350 kHz, the amplitude is 600 V, and the duty cycle is 60%, and the TC4 alloy substrate is etched and cleaned for 20 min.
[0089] Step 4: Introduce high-purity Ar gas with a pressure of 0.5 Pa into the vacuum chamber. When the Al target and the Cr / C target both form a closed magnetic field, and the Cr target and the C target form a mirror magnetic field, turn on the DC power supply of the Al target, and turn on the high-power pulse power supply of the Cr target and the C target at the same time, and use magnetron sputtering to self-clean each target material.
[0090] Step 5: High-purity Ar gas with a pressure of 0.5 Pa is introduced into the vacuum chamber to form a closed magnetic field on both the Al target and the Cr / C target, while the Cr target and the C target form a magnetic pole configuration of a mirror magnetic field. The bias power supply is set and turned on: the frequency is 350 kHz, the negative bias amplitude is 100 V, and the duty cycle is 60%; the Al target DC power supply is turned on with a power of 20 W; at the same time, the high-power pulse power supplies of the Cr target and the C target are turned on, and the powers are set to 65 W and 135 W respectively. The parameters of the HiPIMS power supply are set as follows: frequency, 500 Hz, period 2000 μs, Cr target duty cycle of 2.5%, pulse time 50 μs, C target duty cycle of 5%, pulse time 100 μs, and multi-target magnetron co-sputtering composite pulse negative bias is used to deposit the Cr2AlC MAX phase coating, and the deposition time is 240 min.
[0091] Comparative Example 2:
[0092] This embodiment is a comparative embodiment of the above-mentioned embodiment 2.
[0093] In this embodiment, the substrate is exactly the same as in Example 2, and the polishing, cleaning and surface Ar ion etching cleaning processes of the substrate are also exactly the same. The difference is that in steps 4 and 5, the sputtering of Al, Cr, and C targets all uses a traditional DC magnetron sputtering power supply instead of a high-power pulse power supply, and the DC sputtering source during the deposition process is also set to a constant power of 20W, 65W, and 135W.
[0094] Figure 6 and Figure 7 The X-ray diffraction spectrum and Raman spectrum of the coating obtained in Example 2 and Comparative Example 2 are as follows. Figure 6 and Figure 7 It can be seen that the deposited coating prepared by DC composite dual-target high-power pulsed magnetron sputtering technology is a Cr2AlCMAX phase coating, while the deposited coating prepared by multi-target DC magnetron sputtering in the comparative example is amorphous. There are also some characteristic diffraction peaks from the substrate in the XRD spectrum.
[0095] Figure 8 and Fig. 9 They are the surface morphology images of the coatings obtained in the above-mentioned Example 2 and Comparative Example 2 respectively. Under the assistance of pulsed negative bias, the surface of the deposited coating prepared by the DC composite dual-target high-power pulsed magnetron sputtering technology shows obvious MAX phase layer growth crystallization characteristics. It can be seen from the surface image that the grain size is reduced to a certain extent compared with Example 1. Although the surface of the coating prepared by DC magnetron sputtering can be seen to have the effect of bias-assisted ion bombardment, the surface is still very smooth, showing obvious amorphous coating characteristics.
[0096] Example 3
[0097] In this embodiment, the substrate material is a Ti-6Al-4V alloy sheet, and the specific preparation steps of the Cr2AlC MAX phase coating on the substrate surface are as follows:
[0098] Step 1: Use 400# to 3000# SiC sandpaper to grind the surface of TC4 alloy sheet in turn, and then use 2.5μm diamond polishing agent to polish for 20 minutes.
[0099] Step 2: Place the polished TC4 alloy sheet substrate in acetone and alcohol for ultrasonic cleaning for 10 minutes, then rinse with deionized water, and then blow dry with high-purity N2, and use a metal press to fix the substrate on the rack for use.
[0100] Step 3: Place the rack in the deposition chamber and wait for the mechanical pump and molecular pump to evacuate to 5×10 -4Pa and after the substrate heating temperature reaches 350°C, high-purity Ar gas with a pressure of 2.0 Pa is introduced into the vacuum chamber, and the pulsed negative bias power supply frequency is set to 150 kHz, the amplitude is 400 V, and the duty cycle is 50%. The TC4 alloy substrate is etched and cleaned for 20 min.
[0101] Step 4: Introduce high-purity Ar gas with a pressure of 0.5 Pa into the vacuum chamber. When the Al target and the Cr / C target both form a closed magnetic field, and the Cr target and the C target form a mirror magnetic field, turn on the DC power supply of the Al target, and turn on the high-power pulse power supply of the Cr target and the C target at the same time, and use magnetron sputtering to self-clean each target material.
[0102] Step 5: High-purity Ar gas with a pressure of 0.5 Pa is introduced into the vacuum chamber to form a closed magnetic field on both the Al target and the Cr / C target, while the Cr target and the C target form a magnetic pole configuration of a mirror magnetic field. The bias power supply is set and turned on: the frequency is 150 kHz, the negative bias amplitude is 100 V, and the duty cycle is 50%; the Al target DC power supply is turned on with a power of 15 W; at the same time, the high-power pulse power supplies of the Cr target and the C target are turned on, and the powers are set to 50 W and 100 W respectively. The parameters of the HiPIMS power supply are set as follows: frequency, 100 Hz, period 10000 μs, Cr target duty cycle of 2.5%, pulse time 250 μs, C target duty cycle of 5%, pulse time 500 μs, and multi-target magnetron co-sputtering composite pulse negative bias is used to deposit the Cr2AlC MAX phase coating, and the deposition time is 240 min.
[0103] Example 4
[0104] In this embodiment, the substrate material is a Ti-6Al-4V alloy sheet, and the specific preparation steps of the Cr2AlC MAX phase coating on the substrate surface are as follows:
[0105] Step 1: Use 400# to 3000# SiC sandpaper to grind the surface of TC4 alloy sheet in turn, and then use 2.5μm diamond polishing agent to polish for 20 minutes.
[0106] Step 2: Place the polished TC4 alloy sheet substrate in acetone and alcohol for ultrasonic cleaning for 10 minutes, then rinse with deionized water, and then blow dry with high-purity N2, and use a metal press to fix the substrate on the rack for use.
[0107] Step 3: Place the rack in the deposition chamber and wait for the mechanical pump and molecular pump to evacuate to 5×10 -4Pa and after the substrate heating temperature reaches 350°C, high-purity Ar gas with a pressure of 5.0 Pa is introduced into the vacuum chamber, and the pulsed negative bias power supply frequency is set to 350 kHz, the amplitude is 800 V, and the duty cycle is 70%. The TC4 alloy substrate is etched and cleaned for 20 min.
[0108] Step 4: Introduce high-purity Ar gas with a pressure of 0.5 Pa into the vacuum chamber. When the Al target and the Cr / C target both form a closed magnetic field, and the Cr target and the C target form a mirror magnetic field, turn on the DC power supply of the Al target, and turn on the high-power pulse power supply of the Cr target and the C target at the same time, and use magnetron sputtering to self-clean each target material.
[0109] Step 5: High-purity Ar gas with a pressure of 0.5 Pa is introduced into the vacuum chamber to form a closed magnetic field on both the Al target and the Cr / C target, while the Cr target and the C target form a magnetic pole configuration of a mirror magnetic field. The bias power supply is set and turned on: the frequency is 350 kHz, the negative bias amplitude is 200 V, and the duty cycle is 70%; the Al target DC power supply is turned on with a power of 35 W; at the same time, the high-power pulse power supplies of the Cr target and the C target are turned on, and the powers are set to 100 W and 200 W respectively. The parameters of the HiPIMS power supply are set as follows: frequency, 1000 Hz, period 1000 μs, Cr target duty cycle of 2.5%, pulse time 25 μs, C target duty cycle of 5%, pulse time 50 μs, and multi-target magnetron co-sputtering composite pulse negative bias is used to deposit the Cr2AlC MAX phase coating, and the deposition time is 1200 min.
[0110] Example 5
[0111] In this embodiment, the substrate material is a Ti-6Al-4V alloy sheet, and the specific preparation steps of the Ti2AlC MAX phase coating on the substrate surface are as follows:
[0112] Step 1: Use 400# to 3000# SiC sandpaper to grind the surface of TC4 alloy sheet in turn, and then use 2.5μm diamond polishing agent to polish for 20 minutes.
[0113] Step 2: Place the polished TC4 alloy sheet substrate in acetone and alcohol for ultrasonic cleaning for 10 minutes, then rinse with deionized water, and then blow dry with high-purity N2, and use a metal press to fix the substrate on the rack for use.
[0114] Step 3: Place the rack in the deposition chamber and wait for the mechanical pump and molecular pump to evacuate to 5×10 -4Pa and after the substrate heating temperature reaches 500°C, high-purity Ar gas with a pressure of 2.0 Pa is introduced into the vacuum chamber, and the pulse negative bias power supply frequency is set to 350 kHz, the amplitude is 600 V, and the duty cycle is 60%. The TC4 alloy substrate is etched and cleaned for 20 min.
[0115] Step 4: Introduce high-purity Ar gas with a pressure of 0.5 Pa into the vacuum chamber. Under the magnetic pole configuration in which the Al target and the Ti / C target both form a closed magnetic field, and the Ti target and the C target form a mirror magnetic field, turn on the DC power supply of the Al target, and at the same time turn on the high-power pulse power supply of the Ti target and the C target, and use magnetron sputtering to self-clean each target material.
[0116] Step 5: High-purity Ar gas with a pressure of 0.5 Pa is introduced into the vacuum chamber to form a closed magnetic field on both the Al target and the Ti / C target, while the Ti target and the C target form a magnetic pole configuration of a mirror magnetic field. The bias power supply is set and turned on: the frequency is 350 kHz, the negative bias amplitude is 100 V, and the duty cycle is 60%; the Al target DC power supply is turned on with a power of 25 W; at the same time, the high-power pulse power supplies of the Ti target and the C target are turned on, and the powers are set to 70 W and 140 W respectively. The parameters of the HiPIMS power supply are set as follows: frequency, 500 Hz, period 2000 μs, Ti target duty cycle of 2.5%, pulse time 50 μs, C target duty cycle of 5%, pulse time 100 μs, and multi-target magnetron co-sputtering composite pulse negative bias is used to deposit the Ti2AlC MAX phase coating, and the deposition time is 240 min.
[0117] Example 6
[0118] In this embodiment, the substrate material is a Ti-6Al-4V alloy sheet, and the specific preparation steps of the V2AlC MAX phase coating on the substrate surface are as follows:
[0119] Step 1: Use 400# to 3000# SiC sandpaper to grind the surface of TC4 alloy sheet in turn, and then use 2.5μm diamond polishing agent to polish for 20 minutes.
[0120] Step 2: Place the polished TC4 alloy sheet substrate in acetone and alcohol for ultrasonic cleaning for 10 minutes, then rinse with deionized water, and then blow dry with high-purity N2, and use a metal press to fix the substrate on the rack for use.
[0121] Step 3: Place the rack in the deposition chamber and wait for the mechanical pump and molecular pump to evacuate to 5×10 -4Pa and after the substrate heating temperature reaches 400°C, high-purity Ar gas with a pressure of 2.0 Pa is introduced into the vacuum chamber, and the pulse negative bias power supply frequency is set to 350 kHz, the amplitude is 600 V, and the duty cycle is 60%. The TC4 alloy substrate is etched and cleaned for 20 min.
[0122] Step 4: Introduce high-purity Ar gas with a pressure of 0.5 Pa into the vacuum chamber. When the Al target and the V / C target both form a closed magnetic field, and the V target and the C target form a mirror magnetic field, turn on the DC power supply of the Al target, and at the same time turn on the high-power pulse power supply of the V target and the C target, and use magnetron sputtering to self-clean each target material.
[0123] Step 5: High-purity Ar gas with a pressure of 0.5 Pa is introduced into the vacuum chamber to form a closed magnetic field on both the Al target and the V / C target, and the V target and the C target form a magnetic pole configuration of a mirror magnetic field. The bias power supply is set and turned on: the frequency is 350kHz, the negative bias amplitude is 100V, and the duty cycle is 60%; the Al target DC power supply is turned on with a power of 23W; at the same time, the high-power pulse power supplies of the V target and the C target are turned on, and the powers are set to 65W and 140W respectively. The parameters of the HiPIMS power supply are set as follows: frequency, 500Hz, period 2000μs, V target duty cycle of 2.5%, pulse time 50μs, C target duty cycle of 5%, pulse time 100μs, and multi-target magnetron co-sputtering composite pulse negative bias is used to deposit the V2AlC MAX phase coating, and the deposition time is 240min.
[0124] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0125] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A low temperature preparation method of a MAX phase coating, characterized in that include: providing a substrate; and placing the substrate in a reaction chamber, turning on a DC magnetron sputtering power supply and a high-power pulsed magnetron sputtering power supply, self-cleaning the target material for 20 to 30 minutes, and then using a DC magnetron sputtering composite dual-target high-power pulsed magnetron sputtering technology to deposit a MAX phase coating on the surface of the substrate; Among them, the power of the Al target in the DC magnetron sputtering is 15~35 W, the dual-target target materials used in the dual-target high-power pulsed magnetron sputtering technology are a metal target and a C target, respectively, the metal target is selected from a Cr target or a V target, and the magnetic field between any two targets of the metal target, the C target, and the Al target is a closed magnetic field with opposite magnet polarities or a mirror magnetic field with the same magnet polarity; the power supply parameters of the dual-target high-power pulsed magnetron sputtering technology are set to: frequency of 100~1000 Hz, duty cycle of 2.5~5%, pulse width of 25~500 μs, power of the metal target of 50~100 W, power of the C target of 100~200 W, substrate bias of -200~0 V, and deposition temperature of 350~400 ℃.
2. The low temperature preparation method according to claim 1, characterized in that: The working gas used in the process of forming the MAX phase coating is selected from any one of neon, argon, krypton, and xenon, or a combination of two or more thereof.
3. The low temperature preparation method according to claim 1, characterized in that: Also includes: The substrate was placed in the reaction chamber and vacuumed to 5×10 -4 Pa, the substrate is heated and Ar gas is introduced into the cavity to perform Ar plasma etching and cleaning treatment on the substrate surface.
4. The low temperature preparation method according to claim 3, characterized in that: During the Ar plasma etching and cleaning process, the Ar gas flow rate is 20-50 sccm, the chamber pressure is 2-5 Pa, the substrate negative bias frequency is 150-350 kHz, the amplitude is 400-800 V, and the duty cycle is 50-70%.
5. The low temperature preparation method according to claim 1, characterized in that: Also includes: The substrate is first polished and ultrasonically cleaned; wherein the cleaning liquid used in the ultrasonic cleaning is selected from acetone and / or ethanol.
6. The low temperature preparation method according to claim 1, characterized in that: The matrix is selected from Ti-6Al-4V.
7. A MAX phase coating prepared by the low temperature preparation method according to any one of claims 1 to 6, wherein the atomic ratio in the MAX phase coating is 2:1:1, and the MAX phase coating is selected from any one of Cr2AlC and V2AlC.
8. The MAX phase coating according to claim 7, characterized in that: The purity of the MAX phase coating is greater than 90 wt % and the surface roughness is 10-50 nm.
9. The MAX phase coating according to claim 7, characterized in that: The thickness of the MAX phase coating is 2-10 μm.
10. Use of the MAX phase coating prepared by the low-temperature preparation method according to any one of claims 1 to 6 in the field of protection in high-temperature and severe corrosion environments in the ocean.
Citation Information
Patent Citations
Preparation method of TiAl / Ti2AlC coating with strong combination and high corrosion resistance
CN114717516A