Optical glass and its preparation method and application
By adjusting the proportion of oxide components and production conditions, optical glass with high refractive index, low density, and low expansion coefficient is prepared, which solves the problem of uneven phase separation of existing optical glasses during the molding process and satisfies the requirements for lightness of optical devices. Quantify demand and reduce production costs.
Patent Information
- Application Number
- CN202211715917.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-29
AI Technical Summary
Existing high refractive index optical glass is prone to uneven phase separation during the molding process, resulting in high density and large expansion coefficient, which affects the optical performance, and it is difficult to achieve high refractive index, low density and low expansion coefficient at the same time.
By adjusting the component proportions of SiO2, BaO, Nb2O5, ZrO2, TiO2, La2O3, Bi2O3 and other oxides, and preparing them under specific production conditions, optical glass with a refractive index greater than 1.9 and a density less than 4g/cm3 is produced, combined with a clarifier To improve the stability and processing performance of glass.
The realization of optical glass with high refractive index, low density, low expansion coefficient and uniformity is in line with the development trend of lightweight optical devices, reduces production costs, and improves the difficulty of glass processing and molding and its application prospects.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of glass products, and in particular relates to optical glass and a preparation method and application thereof. Background Art
[0002] In recent years, the market trends of both optical technology and optoelectronic technology (application fields of imaging, projection, laser technology and optical communication engineering technology) have been increasingly moving towards miniaturization, and the optical components used in optical systems are also moving towards miniaturization, lightness and high performance. Optical glass with high refractive index and high dispersion can effectively shorten the total optical length of the lens, miniaturize the imaging system, and is conducive to the development trend of miniaturization of optical devices, because high refractive index optical glass has a very broad application prospect.
[0003] High refractive optical glass is an essential material for AR glasses, eyeglass displays, glasses with projectors, virtual image display devices, etc. In the current market, high refractive index optical glass usually uses a high content of rare earth metal oxides to achieve high refractive effect. However, when a high content of rare earth metal oxides is used, the resulting glass generally has a higher expansion coefficient and a larger density, and is very easy to phase separate during the molding process and difficult to homogenize. The color of the glass appears yellow-brown, which affects the optical properties of the glass.
[0004] Therefore, there is an urgent need in the art for an optical glass that simultaneously satisfies the requirements of high refractive index, low density, and phase homogeneity. Summary of the invention
[0005] In order to solve the problems existing in the above-mentioned prior art, the present invention provides an optical glass. The optical glass prepared by the present invention through the regulation of components and proportions and under certain production conditions has the advantages of high refractive index, low density, low expansion coefficient, not easy to separate phases, high uniformity, etc. The specific contents are as follows:
[0006] In a first aspect, the present invention provides an optical glass, wherein the optical glass composition comprises, by mass percentage, 3% to 50.0% SiO 2 , 0.01%~15.0%Li 2 O+Na 2 O+K 2 O, 6.0% to 35% BaO, 0.01% to 15.0% B 2 O 3 , 10% to 45% Nb 2 O 5 , 0.01%~15% ZrO 2 , 8.5%~35.0% TiO 2 , 5%~55% La2 O 3 , 0.01% ~ 10.0% Bi 2 O 3 +Gd 2 O 3 +Y 2 O 3 , 0%~2.0% CaO, 0%~3.0% SrO, 0%~10.0% ZnO.
[0007] In some embodiments, based on the total weight of the glass composition, the optical glass comprises, by mass percentage, 5% to 47.5% SiO 2 , 0.01%~12%Li 2 O+Na 2 O+K 2 O, 10.5% to 30.5% BaO, 1.1% to 12% B 2 O 3 , 12.5%~37.5% Nb 2 O 5 , 1.0%~13.5% ZrO 2 , 12% to 30% TiO 2 , 10%~50.4% La 2 O 3 , 0.05% ~ 8.5% Bi 2 O 3 +Gd 2 O 3 +Y 2 O 3 , 0.01%~1.7% CaO, 0.01%~2.7% SrO, 0%~10.0% ZnO.
[0008] In some embodiments, the mass percentage of each component is substituted into the formula to calculate Nb 2 O 5 +La 2 O 3 ≥18.5%, and / or ZrO 2 +SiO 2 +B 2 O 3 ≥8%, and / or ZrO 2 +TiO 2 +BaO≥30%; preferably: Nb 2 O 5 +La 2 O 3 ≥23.5.5%, and / or ZrO 2 +SiO 2 +B2 O 3 ≥10%, and / or ZrO 2 +TiO 2 +BaO≥35.5%.
[0009] In some embodiments, the glass composition of the optical glass further includes a clarifier; based on the total weight of the glass composition, the content of the clarifier is 0.01-0.5% by mass.
[0010] In some embodiments, the fining agent is at least one of chloride, fluoride, and sulfide, preferably chloride.
[0011] In some embodiments, the refractive index of the optical glass is greater than 1.9, and / or the visible light transmittance is greater than 85%, and / or the density is less than or equal to 4 g / cm 3 .
[0012] For example, the refractive index of the optical glass may be 1.92, 1.93, 1.95, 1.96, 1.97, 1.98, 2.08 or 2.12, the visible light transmittance may be 85%, 86%, 87%, 88%, 89% or 90%, and the density may be 4 g / cm 3 、3.91g / cm 3 、3.89g / cm 3 、3.87g / cm 3 、3.64g / cm 3 、3.61g / cm 3 、3.58g / cm 3 、3.52g / cm 3 or 3.46 g / cm 3 .
[0013] In some embodiments, the optical glass has a glass liquidus temperature TL less than 1150°C, and / or a glass transition temperature Tg less than or equal to 620°C.
[0014] For example, the glass liquidus temperature TL is 1143°C, 1135°C, 1121°C, 1106°C, 1097°C or 1085°C, and the glass transition temperature Tg may be 620°C, 619°C, 616°C, 615°C, 613°C, 614°C, 609°C, or 608°C.
[0015] In a second aspect, the present invention provides a method for preparing the optical glass described in the first aspect. The method comprises:
[0016] According to the formula ratio, the raw materials are fully stirred and mixed to obtain a batch mixture;
[0017] Melting the batch material mixture at high temperature;
[0018] Casting the molten mixture into a mold and annealing it to obtain a glass sheet;
[0019] The original glass sheets are processed to obtain glass products.
[0020] In some embodiments, the melting temperature is 1200-1500° C., and the time is 3-8 hours; the annealing temperature is 550-630° C., and the time is 1-3 hours.
[0021] For example, the melting temperature can be in the range of 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C and any combination thereof, and the time can be in the range of 3h, 5h, 6h, 7h, 8h and any combination thereof; the annealing temperature can be in the range of 550°C, 570°C, 580°C, 590°C, 600°C, 620°C, 630°C and any combination thereof; the time can be in the range of 1h, 1.5h, 2h, 2.5h, 3h and any combination thereof.
[0022] In a third aspect, the present invention provides an application of the optical glass described in the first aspect.
[0023] The present invention provides an optical glass and a preparation method and application thereof. In terms of mass percentage, the optical glass composition comprises: 3% to 50.0% SiO 2 , 0.01%~15.0%Li 2 O+Na 2 O+K 2 O, 6.0% to 35% BaO, 0.01% to 15.0% B 2 O 3 , 10% to 45% Nb 2 O 5 , 0.01%~15% ZrO 2 , 8.5%~35.0% TiO 2 , 5%~55% La 2 O 3 , 0.01% ~ 10.0% Bi 2 O 3 +Gd 2 O 3 +Y 2 O 3 The optical glass provided by the present invention has a high refractive index and a low density, which conforms to the development trend of lightweight optical devices. At the same time, the glass prepared by the preparation method provided by the present invention is not easy to phase separate, has high uniformity, and is easy to process and shape, which can reduce production costs. Therefore, the optical glass provided by the present invention has broad application prospects. DETAILED DESCRIPTION
[0024] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods. The embodiments of the present invention are described in detail below. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0025] The embodiment of the present invention provides an optical glass. The specific contents are as follows:
[0026] In a first aspect, an embodiment of the present invention provides an optical glass. Based on the total weight of the glass composition, the optical glass composition comprises, in terms of mass percentage, 3% to 50.0% SiO 2 , 0.01%~15.0%Li 2 O+Na 2 O+K 2 O, 6.0% to 35% BaO, 0.01% to 15.0% B 2 O 3 , 10% to 45% Nb 2 O 5 , 0.01%~15% ZrO 2 , 8.5%~35.0% TiO 2 , 5%~55% La 2 O 3 , 0.01% ~ 10.0% Bi 2 O 3 +Gd 2 O 3 +Y 2 O 3 .
[0027] In this embodiment, SiO 2 It is the main network former of glass and a component that improves the stability and chemical durability of glass. 2 The content ratio is 3% to 50%. SiO 2 When the content ratio is 50% or less, a component for obtaining a higher refractive index may be contained. In order to ensure the stability of the glass, SiO 2 The content ratio of SiO is preferably 3% or more, more preferably 5% or more. 2 The content ratio is preferably 50% or less, more preferably 47.5% or less.
[0028] In this embodiment, Li 2 O、Na 2 O.K 2O is an oxide outside the glass structure network. It has the characteristics of reducing the high temperature viscosity of glass and improving the melting performance of glass. It is a good flux for glass and can reduce the glass transition temperature. However, when the alkali metal content is too high, the viscosity curve will become steep, which is not conducive to glass production. Therefore, Li 2 O+Na 2 O+K 2 The content of O is less than or equal to 15.0%, and more preferably, the content of alkali metals is 0.01% to 12%.
[0029] In this embodiment, BaO mainly increases the refractive index. If the content is too low, the refractive index cannot be increased. However, if the content of BaO is large, the density tends to increase. The content of BaO is 6% to 35%, and the content of BaO is preferably 10.5% to 30.5%.
[0030] In this embodiment, B 2 O 3 It can be used as a matrix to form a network structure and can generate glass alone. Its addition can improve the toughness of the glass. 2 O 3 It is also a good flux, which can significantly reduce the melting temperature of glass and is also beneficial to the vitrification process. However, excessive content is not conducive to the improvement of thermal stability and refractive index. Therefore, as mentioned above, B 2 O 3 The content ratio is 0.01 to 15.0%. 2 O 3 The content of is preferably 1.1% to 12%.
[0031] In this embodiment, Nb 2 O 5 It has the function of increasing the high refractive index of the glass and resulting in a smaller Abbe number. If the content is too low, it cannot meet the purpose of increasing the refractive index, but if the content is too high, it can cause the deterioration of the internal transmittance. Therefore, as mentioned above, the Nb content in the composition is 2 O 5 The content of is preferably 10% to 45%, and more preferably 12.5% to 37.5%.
[0032] In this embodiment, ZrO 2 It is a component that increases the refractive index of glass and improves the chemical durability of glass. 2 , can improve the mechanical properties of glass. On the other hand, if ZrO 2 Too much ZrO will cause devitrification. 2 The content ratio is preferably 0.01% to 15.0%, and more preferably 1.0% to 13.5%.
[0033] In this embodiment, TiO2 The main function is to increase the refractive index of glass and increase the dispersion of glass. On the other hand, if TiO 2 Too much will cause coloration, resulting in reduced transmittance, while too little will not achieve the purpose of increasing the refractive index. 2 The content ratio is preferably 8..5% to 35%, and the more preferred content is 12% to 30%.
[0034] In this embodiment, La 2 O 3 It is a component that increases the refractive index of glass. If it is too low, it is impossible to achieve a combination of high refractive index and high Abbe number. However, if La 2 O 3 If the amount of La is too large, the glass viscosity will increase too much and the tendency of devitrification will increase. 2 O 3 The content ratio is preferably 5% to 55%, and more preferably 10% to 50.4%.
[0035] In this embodiment, Gd 2 O 3 It has the effect of increasing the refractive index without reducing the Abbe number. This component is an expensive glass component. At the same time, excessive Gd 2 O 3 Reduce internal transmittance, Bi 2 O 3 It has the effect of significantly increasing the refractive index, because Bi 2 O 3 The inherent color of the glass has an adverse effect on the transmittance of the glass, so it should not be too high. If it is too high, the glass color will become black, resulting in a decrease in transmittance. If it is too low, it will not be able to achieve the purpose of increasing the refractive index. 2 O 3 It has the effect of increasing the refractive index and reducing the high temperature viscosity. 2 O 3 Too high will make the glass easy to crystallize and increase the cost, so it should not be too high. Too low will not achieve the purpose of increasing the refractive index, so Bi 2 O 3 +Gd 2 O 3 +Y 2 O 3 The content of is preferably 0.01% to 10%, and more preferably 0.05% to 8.5%.
[0036] In some embodiments, the refractive index of the optical glass is greater than 1.9, and / or the visible light transmittance is greater than 85%, and / or the density is less than or equal to 4 g / cm 3 .
[0037] For example, the refractive index of the optical glass may be 1.92, 1.93, 1.95, 1.96, 1.97, 1.98, 2.08 or 2.12, the visible light transmittance may be 85%, 86%, 87%, 88%, 89% or 90%, and the density may be 4 g / cm 3 、3.91g / cm 3 、3.89g / cm 3 、3.87g / cm 3 、3.64g / cm 3 、3.61g / cm 3 、3.58g / cm 3 、3.52g / cm 3 or 3.46 g / cm 3 .
[0038] The optical glass provided in the embodiment of the present invention adopts SiO 2 ,BaO,B 2 O 3 , Nb 2 O 5 、ZrO 2 、TiO 2 、Bi 2 O 3 and Gd 2 O 3 , the functions of rare earth metals are coordinated to achieve the purpose of high refractive index. In addition, by uniformly adjusting the content of these oxides, the glass has the characteristics of high refractive index and low density, so as to meet the lightweight development trend of optical devices and reduce the burden on the wearer.
[0039] In some embodiments, the optical glass has a glass liquidus temperature TL less than 1150°C, and / or a glass transition temperature Tg less than or equal to 620°C.
[0040] For example, the glass liquidus temperature TL is 1143°C, 1135°C, 1121°C, 1106°C, 1097°C or 1085°C, and the glass transition temperature Tg may be 620°C, 619°C, 616°C, 615°C, 613°C, 614°C, 609°C, or 608°C.
[0041] The liquidus temperature TL of the optical glass provided by the embodiment of the present invention is less than 1150°C, and the processing difficulty of the glass with a low liquidus temperature is correspondingly low, and it is not easy to lose clarity. Therefore, the optical glass provided by the embodiment of the present invention also has the advantage of low processing difficulty. At the same time, the optical glass provided by the embodiment of the present invention has a low phase separation tendency and high glass uniformity.
[0042] In some embodiments, the mass percentage of each component is substituted into the formula to calculate Nb 2 O 5 +La 2 O 3 ≥18.5%; ZrO 2 +SiO 2 +B 2 O 3 ≥8%; ZrO 2 +TiO 2 +BaO≥30%.
[0043] In the specific implementation, in order to ensure that the material has a high refractive index under the premise of having glass forming ability, in this embodiment, ZrO 2 +SiO 2 +B 2 O 3 ≥8%, which can improve the mechanical properties of glass and reduce the risk of glass devitrification; on the other hand, Nb 2 O 5 +La 2 O 3 ≥18.5%, ZrO 2 +TiO 2 +BaO≥30% can increase the refractive index of glass.
[0044] In some embodiments, preferably, in terms of mass percentage, the mass percentage of each component is substituted into the formula to calculate Nb 2 O 5 +La 2 O 3 ≥23.5%; ZrO 2 +SiO 2 +B 2 O 3 ≥10%; ZrO 2 +TiO 2 +BaO≥35.5%.
[0045] In some embodiments, the optical glass composition further comprises, by mass percentage, 0% to 2.0% CaO.
[0046] In this embodiment, CaO is an oxide outside the glass structure network. CaO is a component that reduces high temperature viscosity without reducing the strain point and significantly improves the solubility. Among alkaline earth metals, CaO is an effective component that increases the Young's modulus of glass without increasing the glass density and the thermal expansion coefficient, second only to MgO. The content of CaO is 0 to 2.0%. If the content is too low, the effect is not obvious. If the content is too high, the glass will become easy to lose clarity and the thermal expansion coefficient will increase significantly. Therefore, the preferred content is 0.01% to 1.7%.
[0047] In some embodiments, the optical glass composition further comprises, by mass percentage, 0% to 3.0% SrO.
[0048] In this embodiment, SrO is a component that improves the melting property of glass, suppresses devitrification, and adjusts the optical constants of glass. On the other hand, when the amount of SrO is too much, devitrification is promoted. The content ratio of SrO is 0 to 3.0%. Therefore, the content ratio of SrO is preferably 0.01% to 2.7%.
[0049] In some embodiments, the optical glass composition further comprises, by mass percentage, 0% to 10.0% ZnO.
[0050] In this embodiment, ZnO can improve the mechanical properties of glass and increase the Young's modulus of glass, while having little effect on the density and thermal expansion coefficient of glass. 2 、TiO 2 ,La 2 O 3 When the amount is too much, the crystallization tendency of the glass will increase. Therefore, the content of ZnO is preferably 0-10%.
[0051] In some embodiments, the glass composition of the optical glass further includes a clarifier; based on the total weight of the glass composition, the content of the clarifier is 0.01-0.5% by mass.
[0052] In this embodiment, the glass composition of the present invention further contains a clarifier, and the content of the clarifier is 0.01-0.5% by mass based on the total weight of the glass composition. In specific implementation, the clarifier is selected from at least one of chloride, fluoride and sulfide, preferably chloride, such as NaCl, NH 4 Cl et al.
[0053] In some embodiments, the glass composition of the optical glass does not contain As 2 O 3 and Sb 2 O 3 .
[0054] As 2 O 3 and Sb 2 O 3 Toxic, in order to avoid harm to human body, the glass composition of this embodiment does not contain As 2 O 3 and Sb 2 O 3 .
[0055] In a second aspect, the present invention provides a method for preparing the optical glass described in the first aspect. The method comprises:
[0056] According to the formula ratio of the first aspect above, the raw materials are fully stirred and mixed to obtain a batch mixture;
[0057] Melting the batch material mixture at high temperature;
[0058] Casting the molten mixture into a mold and annealing it to obtain a glass sheet;
[0059] The original glass sheets are processed to obtain glass products.
[0060] In this embodiment, melting can be carried out in a platinum-rhodium crucible, and the processing temperature is 1200-1500°C for 3-8 hours. For example, the melting temperature can be 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C and any combination thereof, and the time can be 3h, 5h, 6h, 7h, 8h and any combination thereof. Those skilled in the art can determine the specific melting temperature and melting time according to actual conditions, which is well known to those skilled in the art and will not be repeated here.
[0061] According to the method of the present invention, stirring and mixing is a conventional homogenization method in the art, for example, bubbles in the glass liquid can be released by stirring and various components in the glass liquid can be evenly distributed.
[0062] According to the method described in the present invention, casting is a conventional casting molding method in the art, for example, it can be carried out in a stainless steel mold, and the specific steps and condition parameters are well known in the art and will not be repeated here.
[0063] In this embodiment, the annealing temperature is 550°C to 630°C, and the time is 1 to 3 hours. For example, the annealing temperature can be 550°C, 570°C, 580°C, 590°C, 600°C, 620°C, 630°C and any combination thereof; the time can be 1h, 1.5h, 2h, 2.5h, 3h and any combination thereof. Those skilled in the art can determine the specific annealing temperature and annealing time according to actual conditions, which is well known to those skilled in the art and will not be repeated here.
[0064] In this embodiment, there is no particular limitation on the processing, and various common mechanical processing methods in the art may be used. For example, the product obtained by annealing treatment may be sliced, ground, polished, etc., and chemical tempering may also be performed as needed.
[0065] In this embodiment, the chemical strengthening treatment includes one chemical strengthening treatment and / or multiple chemical strengthening treatments. Chemical strengthening is achieved by ion exchange on the surface of the glass plate. The chemical strengthening liquid is sodium nitrate, potassium nitrate and / or a mixed molten liquid of the two. The ion exchange temperature is 390°C to 450°C. Those skilled in the art can determine the specific strengthening temperature and molten salt ratio according to actual conditions. This is well known to those skilled in the art and will not be repeated here.
[0066] The glass prepared by the above preparation method has a refractive index greater than 1.9, a visible light transmittance greater than 85%, and a density less than or equal to 4g / cm 3 The optical glass prepared by the glass composition and preparation method provided by the present invention has a lower expansion coefficient and a smaller density, which conforms to the development trend of lightweight optical devices. At the same time, the glass prepared by the preparation method provided by the present invention is not easy to separate into phases, has high uniformity, and has low difficulty in processing and molding, which can reduce production costs.
[0067] In a third aspect, the present invention provides an application of the optical glass described in the first aspect, which can be applied to various scenarios requiring optical glass, such as AR glasses, glasses-type displays, glasses with projectors, and virtual image display devices.
[0068] In order to make those skilled in the art more clearly understand the technical concept of the present invention, the present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. At the same time, in the following embodiments, unless otherwise specified, the materials used can be obtained commercially, and unless otherwise specified, the methods used are conventional methods in the art. The specific contents are as follows:
[0069] In the following examples and comparative examples, the glass density is measured according to ASTM C-693, and the unit is g / cm 3 .
[0070] The thermal expansion coefficient of glass at 50-350°C is measured using a horizontal dilatometer according to ASTM E-228, in units of 10 -7 / ℃.
[0071] The Young's modulus of glass is measured using a material mechanical testing machine according to ASTM C-623, and the unit is GPa.
[0072] The transmittance of the glass at a wavelength of 550 nm was measured using a UV-2600 ultraviolet-visible spectrophotometer.
[0073] Use WYV-S Digital V Prism Refractometer to test the glass refractive index.
[0074] Tg was measured using a horizontal dilatometer and is reported in °C.
[0075] The high temperature viscosity-temperature curve of glass is measured using a rotational high temperature viscometer in accordance with ASTM C-965, wherein the melting temperature Tm corresponding to the viscosity of 200P is expressed in °C.
[0076] The glass liquidus temperature TL is measured in °C using a gradient furnace method according to ASTM C-829.
[0077] Examples 1-12 and Comparative Examples 1-4 were operated according to the following method to prepare corresponding glass products.
[0078] Weigh each component according to the glass composition shown in Table 1, Table 2, and Table 3, mix well, pour the mixture into a platinum crucible, and then heat it in a high-temperature furnace at 1400℃ for 5 hours, and use a platinum rod to stir to expel bubbles. Pour the molten glass into a stainless steel cast iron mold to form a specified block glass product, and then keep the glass product in an annealing furnace at 600℃ for 2 hours, then reduce it to 300℃ at 1℃ per minute, turn off the power and cool it to room temperature with the furnace. Cut, grind, and polish the glass product, then clean it with deionized water and dry it to obtain a finished glass product. The various properties of each finished glass product were measured, and the results are shown in Table 1, Table 2, and Table 3.
[0079] Table 1. Results of testing various properties of the finished glass products obtained in Examples 1-6
[0080]
[0081] Table 2. Results of testing various properties of the finished glass products obtained in Examples 7-12
[0082]
[0083]
[0084] Table 3. Results of testing various properties of the finished glass products obtained in Comparative Examples 1-4
[0085]
[0086]
[0087] Note: In Table 1-3 above, “--” means: None; “ / ” means: None.
[0088] From the performance test results in Table 1-3 above, we can see that:
[0089] 1. The optical glass provided in this embodiment uses SiO2, BaO, B2O3, Nb2O5, ZrO2, TiO2, Bi2O3 and Gd2O3 to coordinate the functions of rare earth metals, and the refractive index can be as high as 2.08 (as shown in the performance test results of Example 1).
[0090] 2. The optical glass provided in this embodiment can have a lower density by uniformly adjusting the component contents, and its refractive index is as high as 1.96 (as shown in the performance test results of Example 6). In other words, the optical glass provided in this embodiment meets the current lightweight requirements and can reduce the burden on the wearer.
[0091] 3. The optical glasses provided in this embodiment all have a relatively low glass liquidus temperature TL, the lowest of which can be as low as 1085°C (as shown in the performance test results of Example 1), and the highest glass liquidus temperature TL is also less than 1150°C (as shown in the performance test results of Example 3), and the processing difficulty of glass with a low liquidus temperature is correspondingly lower, and it is not easy to lose clarity. Therefore, the optical glass provided in the embodiment of the present invention also has the advantage of low processing difficulty.
[0092] 4. The optical glasses provided in this embodiment all have a relatively low glass transition temperature Tg, the lowest of which can be as low as 608°C (as shown in the performance test results of Example 4), and the highest glass transition temperature Tg is only 620°C (as shown in the performance test results of Example 3). The glass transition temperature (Tg) is the lowest temperature at which a molecular chain segment can move, and its level is directly related to the flexibility of the molecular chain. The greater the flexibility of the molecular chain, the lower the glass transition temperature. Therefore, the optical glass provided in the embodiment of the present invention also has the characteristics of relatively high molecular chain flexibility, thereby further reducing the difficulty of processing and molding.
[0093] 5. As shown in the performance test results of Examples 1-12, when Nb 2 O 5 +La 2 O 3 ≥18.5%, ZrO 2 +SiO 2 +B 2 O 3 ≥8%, ZrO 2 +TiO 2 +BaO≥30%, the prepared optical glass has the advantages of high refractive index, low density, low TL and Tg, low phase separation tendency, high uniformity, etc. 2 O 5 +La 2 O 3 ≥18.5%, ZrO 2 +SiO 2 +B 2 O 3 ≥8%, ZrO 2 +TiO 2+BaO≥30% is not satisfied, the prepared optical glass cannot have the advantages of high refractive index, low density, low TL and Tg, low phase separation tendency, high uniformity, etc. That is to say, the optical glass prepared according to the component requirements provided in this embodiment can meet the current industry needs.
[0094] 6. As shown in the performance test results of Example 1 and Comparative Example 4, if water quenching is not used during the preparation process, the performance of the obtained optical glass is poor. It can be seen that the optical glass component provided in this embodiment, after being prepared by the method provided in this embodiment, has the advantages of high refractive index, low density, low TL and Tg, low phase separation tendency, high uniformity, etc.
[0095] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.
[0096] The optical glass and its preparation method and application provided by the present invention are introduced in detail above. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. An optical glass, characterized in that: The components of the optical glass include, in mass percentage, 3% to 50.0% SiO2, 0.01% to 15.0% Li2O+Na2O+K2O, 6.0% to 35% BaO, 0.01% to 15.0% B2O3, 32.01% to 45% Nb2O5, 0.01% to 15% ZrO2, 8.5% to 35.0% TiO2, 5% to 55% La2O3, 0.01% to 10.0% Bi2O3+Gd2O3+Y2O3, 0% to 2.0% CaO, 0% to 3.0% SrO and 0% to 10.0% ZnO, based on the total weight of the glass composition.
2. The optical glass according to claim 1, characterized in that: The components of the optical glass include, in mass percentage, 5% to 47.5% SiO2, 0.01% to 12% Li2O+Na2O+K2O, 10.5% to 30.5% BaO, 1.1% to 12% B2O3, 32.01% to 37.5% Nb2O5, 1.0% to 13.5% ZrO2, 12% to 30% TiO2, 10% to 50.4% La2O3, 0.05% to 8.5% Bi2O3+Gd2O3+Y2O3, 0.01% to 1.7% CaO, 0.01% to 2.7% SrO and 0% to 10.0% ZnO, based on the total weight of the glass composition.
3. The optical glass according to claim 1, characterized in that: In terms of mass percentage, the mass percentage of each component is substituted into the formula to calculate ZrO2+SiO2+B2O3≥8%, and / or ZrO2+TiO2+BaO≥30%.
4. The optical glass according to claim 1, characterized in that: The glass composition of the optical glass further comprises a clarifier; based on the total weight of the glass composition, the content of the clarifier is 0.01-0.5% by mass.
5. The optical glass according to claim 1, characterized in that: The clarifier is at least one of chloride, fluoride and sulfide.
6. The optical glass according to any one of claims 1 to 5, characterized in that: The optical glass has a refractive index greater than 1.9, and / or a visible light transmittance greater than 85%, and / or a density less than or equal to 4 g / cm 3 .
7. The optical glass according to any one of claims 1 to 5, characterized in that: The optical glass has a glass liquidus temperature TL less than 1150°C, and / or a glass transition temperature Tg less than or equal to 620°C.
8. A method for preparing the optical glass according to any one of claims 1 to 7, characterized in that: include: According to the formula ratio, the raw materials are fully stirred and mixed to obtain a batch mixture; Melting the batch mixture; Casting the molten mixture into a mold and annealing it to obtain a glass sheet; The original glass sheets are processed to obtain glass products.
9. The optical glass according to claim 8, characterized in that: The melting temperature is 1200-1500° C., and the time is 3-8 hours; and / or the annealing temperature is 550-630° C., and the time is 1-3 hours.
10. Use of the optical glass according to any one of claims 1 to 7, characterized in that: The application is any one of AR glasses, glasses-type displays, glasses with a projector, and a virtual image display device.
Citation Information
Patent Citations
Optical glass, glass preform and optical element
CN115231818A
Optical glass, optical element and optical instrument
CN115246707A