A kind of calcium carbonate cement and hardening method and application thereof
Through the combination of amorphous calcium carbonate, vaterite and β-cyclodextrin and the use of crystal form regulators, the crystal form and structure of calcium carbonate cement are regulated, and the problems of high porosity and low compressive strength in calcium carbonate cement are solved. , realizes efficient compression strength improvement and dense structure formation, suitable for low-carbon building materials.
Patent Information
- Application Number
- CN202310172285.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-02-27
AI Technical Summary
The existing calcium carbonate cement has problems of high porosity and low compressive strength, which limits its application scenarios.
Amorphous calcium carbonate, vaterite and β-cyclodextrin or their aqueous solution are used as the main raw materials to prepare calcium carbonate cement by carbonization or precipitation method, and use crystal form regulators such as aragonite whiskers and coral sand and other biomass materials. , regulates the crystal form of calcium carbonate into aragonite, increases the average aspect ratio of aragonite, reduces the porosity, and forms a dense hardened structure.
The compressive strength of calcium carbonate cement hardened body is significantly improved, reaching 10-60MPa, and the porosity is reduced, forming a dense hardened structure, suitable for low-carbon building materials.
Smart Images

Figure CN116239324B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic non-metallic materials, and in particular relates to calcium carbonate cement and a hardening method and application thereof. Background Art
[0002] There are many types of calcium carbonate crystals, with various appearances such as spherical and needle-shaped. Currently known calcium carbonate has various crystal forms such as calcite, aragonite, vaterite, and amorphous calcium carbonate. Among them, amorphous calcium carbonate and vaterite are thermodynamically unstable. Controlling the crystal form transformation of calcium carbonate and accurately controlling the morphological characteristics of calcium carbonate crystals is an important way to prepare calcium carbonate bulk materials. At present, the main way to regulate calcium carbonate crystals is to add inorganic ions or organic matter to affect the lattice or crystal face of calcium carbonate, control its nucleation growth and regulate the physical phase and morphology. Inorganic ions are expensive as crystal form regulators, and organic matter has high storage conditions and is easy to deteriorate, so they cannot be used on a large scale.
[0003] There are various calcium carbonate crystal forms in the current calcium carbonate cement, among which aragonite has a better effect. The reason is that aragonite is needle-shaped, and the three-dimensional network structure it forms produces bonding force, which can form a calcium carbonate hardened body with certain mechanical strength. However, at the same time, the three-dimensional network structure formed by aragonite will produce a large number of pores, and the mechanical properties are poor. The structural characteristics and high porosity of aragonite hinder the improvement of the mechanical properties of calcium carbonate and limit its application scenarios. Now there is an urgent need for a calcium carbonate cement with a large average aspect ratio of aragonite, low porosity, and high compressive strength. Summary of the invention
[0004] In order to overcome the problems existing in the above-mentioned prior art, one of the objects of the present invention is to provide a calcium carbonate cement, which has a dense structure, low porosity and high compressive strength after hardening.
[0005] A second object of the present invention is to provide a method for hardening the above-mentioned calcium carbonate cement.
[0006] A third object of the present invention is to provide a calcium carbonate cement hardened body obtained by the hardening method of the calcium carbonate cement.
[0007] A fourth object of the present invention is to provide an application of the above-mentioned calcium carbonate cement and a hardening method thereof.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] The first aspect of the present invention provides a calcium carbonate cement, comprising the following raw materials in parts by weight: 0 to 400 parts of amorphous calcium carbonate, 200 to 600 parts of vaterite, 10 to 600 parts of a crystal modifier, and 10 to 800 parts of beta-cyclodextrin or its aqueous solution.
[0010] There are many methods for preparing amorphous calcium carbonate, such as decomposition of ammonium carbonate to produce CO 2 Amorphous calcium carbonate can be obtained from various sources, including amorphous calcium carbonate, precipitation method (also known as double decomposition method), carbonization method, etc.
[0011] Among them, the carbonization method of amorphous calcium carbonate is to convert gas CO 2 A method for preparing amorphous calcium carbonate by diffusing into a calcium ion solution such as a calcium salt or a calcium hydroxide solution, wherein the calcium source can be derived from calcium-containing waste resources such as carbide slag, phosphogypsum, and construction solid waste, and is not limited to chemical reagents. 2 It comes from industrial waste gas, can achieve resource recycling, reduce carbon emissions, and has the advantages of simple operation, abundant raw materials, and easy industrial production.
[0012] In a preferred embodiment of the present invention, amorphous calcium carbonate is prepared by a carbonization method.
[0013] Preferably, in the calcium carbonate cement, amorphous calcium carbonate is composed of CO 2 Prepared by reaction with calcium ion solution.
[0014] Preferably, in the calcium carbonate cement, amorphous calcium carbonate is prepared by a method comprising the following steps: 2 A calcium ion solution is introduced, a stabilizer is added, and a carbonization reaction is performed until the pH value of the solution is 7 to 9. The precipitate generated by the reaction is separated and dried to obtain the amorphous calcium carbonate.
[0015] Preferably, the CO 2 The flow rate is 400-600 mL / min; further preferably, the CO 2 The flow rate is 450-550 mL / min; more preferably, the CO 2 The flow rate is 500mL / min.
[0016] Preferably, the calcium ion solution comprises at least one of anhydrous calcium chloride, a hydrate of calcium chloride, anhydrous calcium nitrate, a hydrate of calcium nitrate, anhydrous calcium acetate, a hydrate of calcium acetate or calcium hydroxide; further preferably, the calcium ion solution comprises at least one of a hydrate of calcium chloride, a hydrate of calcium nitrate or a hydrate of calcium acetate; further preferably, the calcium ion solution is selected from calcium chloride dihydrate.
[0017] Preferably, the concentration of the calcium ion solution is 0.8 to 1.2 mol / L; further preferably, the concentration of the calcium ion solution is 0.9 to 1.1 mol / L; preferably, the concentration of the calcium ion solution is 1 mol / L.
[0018] Preferably, the stabilizer includes at least one of magnesium ions, silicate ions, and phosphate ions; further preferably, the stabilizer is selected from magnesium ions; further preferably, the stabilizer is selected from anhydrous magnesium chloride.
[0019] Preferably, the concentration of the stabilizer is 0.08-0.12 mol / L; further preferably, the concentration of the stabilizer is 0.09-0.11 mol / L; further preferably, the concentration of the stabilizer is 0.1 mol / L.
[0020] Preferably, the carbonization reaction is performed until the pH value of the solution is 7.2 to 8.8; further preferably, the carbonization reaction is performed until the pH value of the solution is 7.5 to 8.5; further preferably, the carbonization reaction is performed until the pH value of the solution is 8.
[0021] In another preferred embodiment of the present invention, amorphous calcium carbonate is prepared by a precipitation method.
[0022] Preferably, in the calcium carbonate cement, amorphous calcium carbonate is prepared by reacting a calcium ion solution with a carbonate.
[0023] Preferably, in the calcium carbonate cement, the amorphous calcium carbonate is prepared by a method comprising the following steps: mixing 0.8-1.2 mol / L of a calcium ion solution with 0.08-0.12 mol / L of a carbonate in a volume ratio of 1:(7-11), and then separating and drying the precipitate generated by the reaction to obtain the amorphous calcium carbonate.
[0024] Preferably, in the method for preparing amorphous calcium carbonate, the calcium ion solution includes at least one of anhydrous calcium chloride, a hydrate of calcium chloride, anhydrous calcium nitrate, a hydrate of calcium nitrate, anhydrous calcium acetate or a hydrate of calcium acetate; further preferably, in the method for preparing amorphous calcium carbonate, the calcium ion solution includes at least one of anhydrous calcium chloride, anhydrous calcium nitrate or anhydrous calcium acetate; further preferably, in the method for preparing amorphous calcium carbonate, the calcium ion solution is selected from anhydrous calcium chloride.
[0025] Preferably, in the preparation method of the amorphous calcium carbonate, the carbonate includes at least one of anhydrous sodium carbonate, a hydrate of sodium carbonate, anhydrous sodium bicarbonate, a hydrate of sodium bicarbonate, anhydrous potassium carbonate, a hydrate of potassium carbonate, anhydrous potassium bicarbonate, a hydrate of potassium bicarbonate, anhydrous ammonium carbonate, a hydrate of ammonium carbonate, anhydrous ammonium bicarbonate or a hydrate of ammonium bicarbonate; further preferably, in the preparation method of the amorphous calcium carbonate, the carbonate includes at least one of anhydrous sodium carbonate, anhydrous sodium bicarbonate, anhydrous potassium carbonate, anhydrous potassium bicarbonate, anhydrous ammonium carbonate or anhydrous ammonium bicarbonate; further preferably, in the preparation method of the amorphous calcium carbonate, the carbonate is selected from anhydrous sodium carbonate.
[0026] Preferably, in the method for preparing amorphous calcium carbonate, the concentration of the calcium ion solution is 0.85 to 1.15 mol / L; further preferably, in the method for preparing amorphous calcium carbonate, the concentration of the calcium ion solution is 0.9 to 1.1 mol / L; further preferably, in the method for preparing amorphous calcium carbonate, the concentration of the calcium ion solution is 0.95 to 1.05 mol / L.
[0027] Preferably, in the method for preparing amorphous calcium carbonate, the concentration of carbonate is 0.085-0.115 mol / L; further preferably, in the method for preparing amorphous calcium carbonate, the concentration of carbonate is 0.09-0.11 mol / L; further preferably, in the method for preparing amorphous calcium carbonate, the concentration of carbonate is 0.095-0.105 mol / L.
[0028] Preferably, in the method for preparing amorphous calcium carbonate, the volume ratio of calcium ion solution to carbonate is 1:(7.5-10.5); further preferably, in the method for preparing amorphous calcium carbonate, the volume ratio of calcium ion solution to carbonate is 1:(8-10); further preferably, in the method for preparing amorphous calcium carbonate, the volume ratio of calcium ion solution to carbonate is 1:(8.5-9.5).
[0029] Preferably, in the method for preparing amorphous calcium carbonate, the separation includes at least one of filtration, suction filtration or centrifugation; further preferably, in the method for preparing amorphous calcium carbonate, the separation includes at least one of filtration or suction filtration; even further preferably, in the method for preparing amorphous calcium carbonate, the separation is selected from suction filtration.
[0030] Preferably, in the method for preparing amorphous calcium carbonate, the drying temperature is 40 to 80°C; further preferably, in the method for preparing amorphous calcium carbonate, the drying temperature is 50 to 70°C; further preferably, in the method for preparing amorphous calcium carbonate, the drying temperature is 55 to 65°C.
[0031] Preferably, in the method for preparing amorphous calcium carbonate, the drying time is 12 to 36 hours; further preferably, in the method for preparing amorphous calcium carbonate, the drying time is 18 to 30 hours; further preferably, in the method for preparing amorphous calcium carbonate, the drying time is 22 to 26 hours.
[0032] Preferably, in the preparation method of amorphous calcium carbonate, the precipitate is washed after separation and before drying; further preferably, the washing solvent includes at least one of water and an organic solvent; further preferably, the washing solvent is deionized water and anhydrous ethanol.
[0033] Preferably, the purity of amorphous calcium carbonate in the calcium carbonate cement is 90-100%; further preferably, the purity of amorphous calcium carbonate in the calcium carbonate cement is 94-100%; further preferably, the purity of amorphous calcium carbonate in the calcium carbonate cement is 98-100%.
[0034] There are also many preparation methods for vaterite, such as thermal decomposition, precipitation, carbonization, etc. It can be seen that there are many sources for obtaining vaterite.
[0035] Among them, the carbonization method of vaterite is similar to the carbonization method of amorphous calcium carbonate, both of which use gas CO 2 The reaction is carried out by diffusion into calcium ion solutions such as calcium salt or calcium hydroxide solution. The specific experimental conditions are different. The calcium ion-containing solution can also come from waste resources such as carbide slag, phosphogypsum, and construction solid waste, rather than being limited to chemical reagents. CO 2 It can also come from industrial waste gas, which can achieve resource recycling and reduce carbon emissions. It also has the advantages of simple operation, abundant raw materials, and easy industrial production.
[0036] In a preferred embodiment of the present invention, vaterite is prepared by carbonization method.
[0037] Preferably, in the calcium carbonate cement, vaterite is composed of CO 2 It is prepared by the reaction of aqueous ammonia and calcium ion solution.
[0038] Preferably, in the calcium carbonate cement, vaterite is prepared by a method comprising the following steps: adding ammonia water to a calcium ion solution, introducing CO 2 When the pH value of the solution is 7-9, the precipitate generated by the reaction is separated and dried to obtain the vaterite.
[0039] Preferably, the calcium ion solution includes at least one of anhydrous calcium chloride, a hydrate of calcium chloride, anhydrous calcium nitrate, a hydrate of calcium nitrate, anhydrous calcium acetate, a hydrate of calcium acetate or calcium hydroxide; further preferably, the calcium ion solution includes at least one of anhydrous calcium chloride, anhydrous calcium nitrate or anhydrous calcium acetate; further preferably, the calcium ion solution is selected from anhydrous calcium chloride.
[0040] Preferably, the concentration of the calcium ion solution is 0.1-0.2 mol / L; further preferably, the concentration of the calcium ion solution is 0.12-0.18 mol / L; preferably, the concentration of the calcium ion solution is 0.15 mol / L.
[0041] Preferably, the concentration of the ammonia water is 25-28 wt %; further preferably, the concentration of the ammonia water is 26-27 wt %; further preferably, the concentration of the ammonia water is 26 wt %.
[0042] Preferably, the amount of ammonia water added is 1-6% of the volume of the calcium ion solution; further preferably, the amount of ammonia water added is 2-5% of the volume of the calcium ion solution; further preferably, the amount of ammonia water added is 3-4% of the volume of the calcium ion solution.
[0043] Preferably, the CO 2 The flow rate is 500-700 mL / min; further preferably, the CO 2 The flow rate is 550-650 mL / min; more preferably, the CO 2 The flow rate is 600mL / min.
[0044] Preferably, CO is introduced 2 to a pH of 7.2 to 8.8; preferably, CO is introduced 2 to a pH of 7.5 to 8.5; more preferably, CO is introduced 2 until the pH of the solution is 8.
[0045] In another preferred embodiment of the present invention, vaterite is prepared by a precipitation method.
[0046] Preferably, in the calcium carbonate cement, vaterite is prepared by the reaction of a calcium ion solution and a carbonate.
[0047] Preferably, in the calcium carbonate cement, vaterite is prepared by a method comprising the following steps: mixing 1.8-2.2 mol / L of calcium ion solution and 1.8-2.2 mol / L of carbonate in an equal volume ratio, and then separating and drying the precipitate generated by the reaction to obtain the vaterite.
[0048] Preferably, in the method for preparing vaterite, the calcium ion solution includes at least one of anhydrous calcium chloride, a hydrate of calcium chloride, anhydrous calcium nitrate, a hydrate of calcium nitrate, anhydrous calcium acetate or a hydrate of calcium acetate; further preferably, in the method for preparing vaterite, the calcium ion solution includes at least one of a hydrate of calcium chloride, a hydrate of calcium nitrate or a hydrate of calcium acetate; further preferably, in the method for preparing vaterite, the calcium ion solution is selected from calcium chloride dihydrate.
[0049] Preferably, in the preparation method of vaterite, the carbonate includes at least one of anhydrous sodium carbonate, a hydrate of sodium carbonate, anhydrous sodium bicarbonate, a hydrate of sodium bicarbonate, anhydrous potassium carbonate, a hydrate of potassium carbonate, anhydrous potassium bicarbonate, a hydrate of potassium bicarbonate, anhydrous ammonium carbonate, a hydrate of ammonium carbonate, anhydrous ammonium bicarbonate or a hydrate of ammonium bicarbonate; further preferably, in the preparation method of vaterite, the carbonate includes at least one of anhydrous sodium carbonate, anhydrous sodium bicarbonate, anhydrous potassium carbonate, anhydrous potassium bicarbonate, anhydrous ammonium carbonate or anhydrous ammonium bicarbonate; further preferably, in the preparation method of vaterite, the carbonate is selected from anhydrous potassium carbonate.
[0050] Preferably, in the method for preparing vaterite, the concentration of the calcium ion solution is 1.85 to 2.15 mol / L; further preferably, in the method for preparing vaterite, the concentration of the calcium ion solution is 1.9 to 2.1 mol / L; further preferably, in the method for preparing vaterite, the concentration of the calcium ion solution is 1.95 to 2.05 mol / L.
[0051] Preferably, in the method for preparing vaterite, the concentration of carbonate is 1.85 to 2.15 mol / L; further preferably, in the method for preparing vaterite, the concentration of carbonate is 1.9 to 2.1 mol / L; further preferably, in the method for preparing vaterite, the concentration of carbonate is 1.95 to 2.05 mol / L.
[0052] Preferably, in the method for preparing vaterite, the separation includes at least one of filtration, suction filtration or centrifugation; further preferably, in the method for preparing vaterite, the separation includes at least one of filtration or suction filtration; even further preferably, in the method for preparing vaterite, the separation is selected from suction filtration.
[0053] Preferably, in the method for preparing vaterite, the drying temperature is 40 to 80°C; further preferably, in the method for preparing vaterite, the drying temperature is 50 to 70°C; further preferably, in the method for preparing vaterite, the drying temperature is 55 to 65°C.
[0054] Preferably, in the method for preparing vaterite, the drying time is 12 to 36 hours; further preferably, in the method for preparing vaterite, the drying time is 18 to 30 hours; further preferably, in the method for preparing vaterite, the drying time is 22 to 26 hours.
[0055] Preferably, in the method for preparing vaterite, the precipitate is washed after being separated and before being dried; further preferably, the washing solvent includes at least one of water and an organic solvent; further preferably, the washing solvent is deionized water and anhydrous ethanol.
[0056] Preferably, in the calcium carbonate cement, the purity of vaterite is 90-100%; further preferably, in the calcium carbonate cement, the purity of vaterite is 92-100%; further preferably, in the calcium carbonate cement, the purity of vaterite is 95-100%.
[0057] Preferably, in the calcium carbonate cement, the crystal form regulator includes at least one of aragonite whiskers, coral sand or shell powder, and the crystal form regulator is selected from these biomass materials containing aragonite minerals; further preferably, in the calcium carbonate cement, the crystal form regulator includes at least one of aragonite whiskers or coral sand; further preferably, in the calcium carbonate cement, the crystal form regulator is selected from coral sand.
[0058] Preferably, in the calcium carbonate cement, in the crystal form regulator, the average aspect ratio of the aragonite whiskers is 5 to 40; further preferably, in the calcium carbonate cement, in the crystal form regulator, the average aspect ratio of the aragonite whiskers is 7 to 30; further preferably, in the calcium carbonate cement, in the crystal form regulator, the average aspect ratio of the aragonite whiskers is 9 to 20.
[0059] Preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of the aragonite whiskers is 85 to 100 wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of the aragonite whiskers is 90 to 100 wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of the aragonite whiskers is 98 to 100 wt%.
[0060] Preferably, in the calcium carbonate cement and the crystal form regulator, the average particle size of the coral sand is 20 to 300 μm; further preferably, in the calcium carbonate cement and the crystal form regulator, the average particle size of the coral sand is 40 to 100 μm; further preferably, in the calcium carbonate cement and the crystal form regulator, the average particle size of the coral sand is 60 to 80 μm.
[0061] Preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of coral sand is 75-100wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of coral sand is 85-98wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of coral sand is 95-97wt%.
[0062] Preferably, in the calcium carbonate cement, in the crystal form regulator, the average particle size of the shell powder is 25 to 300 μm; further preferably, in the calcium carbonate cement, in the crystal form regulator, the average particle size of the shell powder is 30 to 200 μm; further preferably, in the calcium carbonate cement, in the crystal form regulator, the average particle size of the shell powder is 40 to 50 μm.
[0063] Preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of shell powder is 70 to 100 wt%; further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of shell powder is 80 to 95 wt%; even further preferably, in the calcium carbonate cement, in the crystal form regulator, the aragonite content of shell powder is 92 to 94 wt%.
[0064] Preferably, the mass fraction of amorphous calcium carbonate in the calcium carbonate cement is 50 to 400 parts; further preferably, the mass fraction of amorphous calcium carbonate in the calcium carbonate cement is 100 to 300 parts; further preferably, the mass fraction of amorphous calcium carbonate in the calcium carbonate cement is 200 to 300 parts.
[0065] Preferably, the mass fraction of vaterite in the calcium carbonate cement is 200-550 parts; further preferably, the mass fraction of vaterite in the calcium carbonate cement is 200-500 parts; further preferably, the mass fraction of vaterite in the calcium carbonate cement is 200-300 parts.
[0066] Preferably, in the calcium carbonate cement, the mass fraction of the crystal form regulator is 100 to 550 parts; further preferably, in the calcium carbonate cement, the mass fraction of the crystal form regulator is 200 to 500 parts; further preferably, in the calcium carbonate cement, the mass fraction of the crystal form regulator is 300 to 500 parts.
[0067] Preferably, the calcium carbonate cement comprises the following raw materials in parts by mass: 50 to 400 parts of amorphous calcium carbonate, 200 to 600 parts of vaterite, 10 to 600 parts of a crystal modifier, and 10 to 800 parts of β-cyclodextrin or its aqueous solution.
[0068] Preferably, the mass fraction of β-cyclodextrin in the calcium carbonate cement is 10 to 80 parts; further preferably, the mass fraction of β-cyclodextrin in the calcium carbonate cement is 12 to 70 parts; further preferably, the mass fraction of β-cyclodextrin in the calcium carbonate cement is 15 to 65 parts.
[0069] Preferably, the calcium carbonate cement comprises the following raw materials in parts by weight: 0 to 400 parts of amorphous calcium carbonate, 200 to 600 parts of vaterite, 10 to 600 parts of a crystal form regulator, and 10 to 80 parts of β-cyclodextrin.
[0070] Further preferably, the calcium carbonate cement comprises the following raw materials in parts by mass: 50 to 400 parts of amorphous calcium carbonate, 200 to 550 parts of vaterite, 100 to 550 parts of crystal modifier, and 10 to 80 parts of β-cyclodextrin.
[0071] More preferably, the calcium carbonate cement comprises the following raw materials in parts by mass: 100-300 parts of amorphous calcium carbonate, 200-500 parts of vaterite, 200-500 parts of crystal modifier, and 12-70 parts of β-cyclodextrin.
[0072] More preferably, the calcium carbonate cement comprises the following raw materials in parts by weight: 200-300 parts of amorphous calcium carbonate, 200-300 parts of vaterite, 300-500 parts of crystal modifier, and 15-65 parts of β-cyclodextrin.
[0073] Preferably, the mass fraction of the β-cyclodextrin aqueous solution in the calcium carbonate cement is 40 to 800 parts; further preferably, the mass fraction of the β-cyclodextrin aqueous solution in the calcium carbonate cement is 80 to 640 parts; further preferably, the mass fraction of the β-cyclodextrin aqueous solution in the calcium carbonate cement is 100 to 560 parts.
[0074] Preferably, the concentration of the β-cyclodextrin aqueous solution in the calcium carbonate cement is 1 to 30 wt %; further preferably, the concentration of the β-cyclodextrin aqueous solution in the calcium carbonate cement is 3 to 25 wt %; further preferably, the concentration of the β-cyclodextrin aqueous solution in the calcium carbonate cement is 5 to 20 wt %.
[0075] Preferably, the calcium carbonate cement comprises the following raw materials in parts by weight: 0 to 400 parts of amorphous calcium carbonate, 200 to 600 parts of vaterite, 10 to 600 parts of a crystal form regulator, and 40 to 800 parts of a β-cyclodextrin aqueous solution.
[0076] Further preferably, the calcium carbonate cement comprises the following raw materials in parts by mass: 50-400 parts of amorphous calcium carbonate, 200-550 parts of vaterite, 100-550 parts of crystal modifier, and 40-800 parts of β-cyclodextrin aqueous solution.
[0077] More preferably, the calcium carbonate cement comprises the following raw materials in parts by mass: 100-300 parts of amorphous calcium carbonate, 200-500 parts of vaterite, 200-500 parts of crystal modifier, and 80-640 parts of β-cyclodextrin aqueous solution.
[0078] More preferably, the calcium carbonate cement comprises the following raw materials in parts by weight: 200-300 parts of amorphous calcium carbonate, 200-300 parts of vaterite, 300-500 parts of crystal modifier, and 100-560 parts of β-cyclodextrin aqueous solution.
[0079] Preferably, the raw materials of the calcium carbonate cement also include water.
[0080] Preferably, in the calcium carbonate cement, the mass ratio of liquid to solid is 0.1 to 0.5; further preferably, in the calcium carbonate cement, the mass ratio of liquid to solid is 0.2 to 0.4; further preferably, in the calcium carbonate cement, the mass ratio of liquid to solid is 0.25 to 0.35. Wherein, since β-cyclodextrin is soluble in water, in the calcium carbonate cement, the liquid includes water and β-cyclodextrin, and the solid includes vaterite and a crystal form regulator, or amorphous calcium carbonate, vaterite and a crystal form regulator.
[0081] The second aspect of the present invention provides a method for hardening the calcium carbonate cement described in the first aspect of the present invention, the hardening method comprising the following steps: mixing the raw materials, and then molding and curing to obtain a hardened body of the calcium carbonate cement.
[0082] Preferably, in the hardening method, vaterite and a crystal form regulator, or amorphous calcium carbonate, vaterite and a crystal form regulator are first mixed to obtain a solid raw material, and then a β-cyclodextrin aqueous solution is added to obtain a calcium carbonate cement slurry, and the calcium carbonate cement slurry is molded and cured to obtain a hardened body of the calcium carbonate cement.
[0083] Preferably, in the hardening method, β-cyclodextrin is mixed with water to obtain a β-cyclodextrin aqueous solution, which is then mixed with other raw materials.
[0084] Preferably, in the hardening method, the concentration of the β-cyclodextrin aqueous solution is 1 to 30 wt%; further preferably, in the calcium carbonate cement, the concentration of the β-cyclodextrin aqueous solution is 3 to 25 wt%; further preferably, in the hardening method, the concentration of the β-cyclodextrin aqueous solution is 5 to 20 wt%.
[0085] Preferably, in the hardening method, amorphous calcium carbonate and vaterite are first mixed to prepare a calcium carbonate cement precursor, and then a crystal modifier is added and mixed to obtain a solid raw material.
[0086] Preferably, in the hardening method, the mixing time of amorphous calcium carbonate and vaterite is 1 to 8 minutes; further preferably, in the hardening method, the mixing time of amorphous calcium carbonate and vaterite is 2 to 6 minutes; further preferably, in the hardening method, the mixing time of amorphous calcium carbonate and vaterite is 2 to 4 minutes.
[0087] Preferably, in the hardening method, the mixing time for adding the crystal form regulator for mixing is 2 to 10 minutes; further preferably, in the hardening method, the mixing time for adding the crystal form regulator for mixing is 3 to 8 minutes; further preferably, in the hardening method, the mixing time for adding the crystal form regulator for mixing is 4 to 6 minutes.
[0088] Preferably, in the hardening method, the molding includes at least one of extrusion molding, casting molding, and press molding.
[0089] Preferably, in the hardening method, the molding pressure is 0 to 200 MPa; further preferably, in the hardening method, the molding pressure is 50 to 150 MPa; further preferably, in the hardening method, the molding pressure is 50 to 100 MPa.
[0090] Preferably, in the hardening method, the curing includes at least one of air curing, water curing or steam curing.
[0091] Preferably, in the hardening method, the curing time is 1 to 5 days; further preferably, in the hardening method, the curing time is 1 to 3 days; further preferably, in the hardening method, the curing time is 1 to 2 days.
[0092] Preferably, in the hardening method, the curing temperature is 20 to 100°C; further preferably, in the hardening method, the curing temperature is 30 to 90°C; further preferably, in the hardening method, the curing temperature is 40 to 80°C.
[0093] The third aspect of the present invention provides a hardened calcium carbonate cement body obtained by the hardening method of calcium carbonate cement according to the second aspect of the present invention.
[0094] Preferably, the average aspect ratio of aragonite in the hardened calcium carbonate cement body is 8-20; further preferably, the average aspect ratio of aragonite in the hardened calcium carbonate cement body is 9-18; further preferably, the average aspect ratio of aragonite in the hardened calcium carbonate cement body is 9-15.
[0095] Preferably, the porosity of the hardened calcium carbonate cement body is 30-40%; further preferably, the porosity of the hardened calcium carbonate cement body is 31-38%; further preferably, the porosity of the hardened calcium carbonate cement body is 32-36%.
[0096] The fourth aspect of the present invention provides the calcium carbonate cement described in the first aspect of the present invention, or the hardening method of the calcium carbonate cement described in the second aspect of the present invention, or the application of the hardened calcium carbonate cement described in the third aspect of the present invention in the field of building materials.
[0097] Preferably, the field of building materials is the field of low-carbon building materials.
[0098] The beneficial effects of the present invention are as follows: the present invention uses a crystal form regulator to regulate the thermodynamically unstable calcium carbonate crystal form to transform it into aragonite, and then uses beta-cyclodextrin to modify the structure of the calcium carbonate, thereby increasing the average aspect ratio of the aragonite, reducing the porosity of the block, forming a dense hardened structure, and significantly improving the compressive strength of the hardened calcium carbonate cement body.
[0099] Specifically, the present invention has the following advantages compared with the prior art:
[0100] 1. β-cyclodextrin is a cylindrical molecule composed of 7 glucose groups connected by 1,4-glycosidic bonds. It has a wide range of applications and low production costs. It is the most widely used cyclodextrin product in industry and can undergo inclusion reaction with calcium carbonate through non-covalent bonds between molecules. Since multiple branching points are formed during the polymerization process to form a three-dimensional network structure, β-cyclodextrin has the characteristics of good mechanical strength, good stability and chemical adjustability. The present invention adds β-cyclodextrin to the uncoagulated calcium carbonate cement powder, and utilizes the -OH in the β-cyclodextrin molecule to react with the Ca in the calcium carbonate. 2+ The electrostatic interaction between β-cyclodextrin molecules and calcium carbonate lattice produces geometric matching and stereochemical complementarity, which affects the nucleation and growth of aragonite in calcium carbonate cement, thereby increasing the average aspect ratio of aragonite, reducing porosity, and forming a dense hardened structure. The compressive strength of the hardened calcium carbonate cement can reach 10 to 60 MPa.
[0101] 2. Both amorphous calcium carbonate and vaterite are thermodynamically unstable calcium carbonate crystal forms, and can be converted into rod-shaped aragonite through the regulation of crystal form regulators. Among them, amorphous calcium carbonate is more active and is easier to convert into aragonite than vaterite, which is beneficial to the reaction process, but has little effect on mechanical properties.
[0102] 3. The present invention uses biomass materials containing aragonite minerals such as aragonite whiskers, coral sand, and shell powder as crystal form regulators, which can induce the formation of aragonite inside calcium carbonate cement and further improve the pore structure and compressive strength of calcium carbonate cement.
[0103] 4. The calcium carbonate cement provided by the present invention has a wide range of raw materials and low cost, and is a low-carbon cement material with high strength. Its hardening method is also simple and easy, so it has a wide range of applications in the field of building materials, especially the field of low-carbon building materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0104] Figure 1 1 is the XRD diagram of amorphous calcium carbonate and vaterite in the examples and comparative examples.
[0105] Figure 2 These are infrared images of the hardened calcium carbonate cement bodies of Examples 1 to 4 and Comparative Examples 1 to 2 cured for one day.
[0106] Figure 3 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 1.
[0107] Figure 4 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 2.
[0108] Figure 5 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 3.
[0109] Figure 6 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 4.
[0110] Figure 7 This is the SEM image of the hardened calcium carbonate cement body of Comparative Example 1 cured for 1 day.
[0111] Figure 8 This is the SEM image of the hardened calcium carbonate cement body of Comparative Example 2 cured for 1 day. DETAILED DESCRIPTION
[0112] The content of the present invention is further described in detail below through specific examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the principles set forth in the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific data exemplified below. The raw materials, reagents or devices used in the following examples and comparative examples, unless otherwise specified, can all be obtained from conventional commercial sources, or can be obtained by existing known methods.
[0113] The amorphous calcium carbonate and vaterite used in the examples and comparative examples of the present invention are both prepared by precipitation method.
[0114] The preparation method of amorphous calcium carbonate is as follows: 1 mol / L anhydrous calcium chloride and 0.1 mol / L sodium carbonate are mixed in a volume ratio of 1:9, the precipitate is immediately filtered, the filter cake is washed with deionized water and anhydrous ethanol, and then dried at 60°C for 24 hours.
[0115] The preparation method of vaterite is as follows: after mixing 2.0 mol / L of equal volume and concentration of calcium chloride dihydrate and anhydrous potassium carbonate, the precipitate is filtered, the filter cake is washed with deionized water and anhydrous ethanol and then dried at 60° C. for 24 hours.
[0116] XRD was used to characterize the products of amorphous calcium carbonate and vaterite. The XRD patterns are shown in Figure 1 As shown, the purity of amorphous calcium carbonate is 100% and the purity of vaterite is 98%.
[0117] The average aspect ratio of the aragonite whiskers used in the embodiments of the present invention and the comparative examples is 10, and the aragonite content is 99wt%; the average particle size of the coral sand is 80μm, and the aragonite content is 97wt%; the average particle size of the shell powder is 50μm, and the aragonite content is 94wt%.
[0118] Example 1
[0119] A calcium carbonate cement comprises the following raw materials in parts by weight: 200 parts of amorphous calcium carbonate, 300 parts of vaterite, 50 parts of aragonite whiskers and 15.75 parts of beta-cyclodextrin.
[0120] The hardening method of the calcium carbonate cement is as follows: 200 parts of amorphous calcium carbonate and 300 parts of vaterite are mixed in a stirring pot, stirred for 3 minutes, and then 400 parts of aragonite whiskers are added and stirred for 5 minutes to obtain a solid raw material. A β-cyclodextrin solution with a concentration of 5wt% is configured, and it is mixed with the solid raw material according to a liquid-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20mm, and an automatic press is used for pressurization, and the molding pressure is 100MPa. After pressurization for 2 minutes, the demolding is performed to obtain a test block with a height of 20mm and a diameter of 20mm, and the test block is placed in a steam environment with a temperature of 60°C for curing to obtain a hardened body of the calcium carbonate cement.
[0121] Example 2
[0122] A calcium carbonate cement comprises the following raw materials in parts by weight: 300 parts of amorphous calcium carbonate, 200 parts of vaterite, 200 parts of shell powder and 31.5 parts of beta-cyclodextrin.
[0123] The hardening method of the calcium carbonate cement is as follows: 300 parts of amorphous calcium carbonate and 200 parts of vaterite are mixed in a stirring pot, stirred for 3 minutes, and then 400 parts of shell powder are added and stirred for 5 minutes to obtain a solid raw material. A β-cyclodextrin solution with a concentration of 10wt% is configured, and it is mixed with the solid raw material according to a liquid-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20mm, and an automatic press is used for pressurization, and the molding pressure is 100MPa. After pressurization for 2 minutes, demolding is performed to obtain a test block with a height of 20mm and a diameter of 20mm, and the test block is placed in a steam environment with a temperature of 80°C for curing to obtain a hardened body of the calcium carbonate cement.
[0124] Example 3
[0125] A calcium carbonate cement comprises the following raw materials in parts by weight: 100 parts of amorphous calcium carbonate, 300 parts of vaterite, 500 parts of coral sand and 47.25 parts of beta-cyclodextrin.
[0126] The hardening method of the calcium carbonate cement is as follows: 100 parts of amorphous calcium carbonate and 300 parts of vaterite are mixed in a stirring pot, stirred for 3 minutes, and then 500 parts of coral sand are added and stirred for 5 minutes to obtain a solid raw material. A 15wt% β-cyclodextrin solution is prepared, and it is mixed with the solid raw material at a liquid-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, and the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and an automatic press is used for pressurization, and the molding pressure is 100 MPa. After pressurization for 2 minutes, the mold is demolded to obtain a test block with a height of 20 mm and a diameter of 20 mm, and the test block is placed in a steam environment at a temperature of 40°C for curing to obtain a hardened body of the calcium carbonate cement.
[0127] Example 4
[0128] A calcium carbonate cement comprises the following raw materials in parts by weight: 500 parts of vaterite, 400 parts of coral sand and 63 parts of beta-cyclodextrin.
[0129] The hardening method of the calcium carbonate cement is as follows: 500 parts of vaterite and 300 parts of coral sand are mixed in a stirring pot and stirred for 5 minutes to obtain a solid raw material. A 20wt% β-cyclodextrin solution is prepared and mixed with the solid raw material at a liquid-to-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and an automatic press is used for pressurization at a molding pressure of 100 MPa. After pressurization for 2 minutes, the mold is removed to obtain a test block with a height of 20 mm and a diameter of 20 mm, and the test block is placed in a steam environment at a temperature of 60° C. for curing to obtain a hardened body of the calcium carbonate cement.
[0130] Comparative Example 1
[0131] A calcium carbonate cement comprises the following raw materials in parts by mass: 300 parts of amorphous calcium carbonate, 200 parts of vaterite and 400 parts of shell powder.
[0132] The hardening method of the calcium carbonate cement is as follows: 300 parts of amorphous calcium carbonate and 200 parts of vaterite are mixed in a stirring pot, stirred for 3 minutes, and then 400 parts of shell powder are added and stirred for 5 minutes to obtain a solid raw material. Water is mixed with the solid raw material at a liquid-to-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and an automatic press is used for pressurization, the molding pressure is 100 MPa, and the demolding is performed after pressurization for 2 minutes to obtain a test block with a height of 20 mm and a diameter of 20 mm, and the test block is placed in a steam environment at a temperature of 80° C. for curing to obtain a hardened body of the calcium carbonate cement.
[0133] Comparative Example 2
[0134] A calcium carbonate cement comprises the following raw materials in parts by mass: 200 parts of amorphous calcium carbonate and 300 parts of vaterite.
[0135] The hardening method of the calcium carbonate cement is as follows: 200 parts of amorphous calcium carbonate and 300 parts of vaterite are mixed in a stirring pot and stirred for 3 minutes to obtain a solid raw material. Water is mixed with the solid raw material at a liquid-to-solid ratio of 0.35 to obtain a calcium carbonate cement slurry, the slurry is poured into a stainless steel cylindrical mold with a diameter of 20 mm, and an automatic press is used for pressurization at a molding pressure of 100 MPa. After pressurization for 2 minutes, the mold is demolded to obtain a test block with a height of 20 mm and a diameter of 20 mm, and the test block is placed in a steam environment at a temperature of 60° C. for curing to obtain a hardened body of the calcium carbonate cement.
[0136] Performance Testing
[0137] 1) The compressive strength of the hardened calcium carbonate cement obtained in Examples 1 to 4 and Comparative Examples 1 to 2 was tested using an electronic universal testing machine at a loading speed of 1 mm / min. The 1-day compressive strength is the compressive strength of the hardened calcium carbonate cement after curing for 1 day, and the 28-day compressive strength is the compressive strength of the hardened calcium carbonate cement after curing for 28 days.
[0138] 2) The setting time, average aspect ratio of aragonite and porosity of the calcium carbonate cement obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were tested. The setting time is the curing time required for amorphous calcium carbonate and vaterite to be completely transformed into aragonite. XRD and infrared were used to determine the phase composition of calcium carbonate at different curing times. When the crystal transformation is completed, the curing is complete, and the curing time is the setting time; the average aspect ratio of aragonite is measured based on the rod-shaped aragonite in the SEM image; the porosity is obtained based on the mercury injection method.
[0139] 3) Infrared images and SEM images of the hardened calcium carbonate cement bodies of test examples 1 to 4 and comparative examples 1 to 2.
[0140] The test results are recorded in Table 1.
[0141] Table 1 Test results of Examples 1 to 4 and Comparative Examples 1 to 2
[0142]
[0143] The compressive strength and average aspect ratio of aragonite in the hardened calcium carbonate cement obtained in Examples 1 to 4 are higher than those in Comparative Example 1. Comparative Example 2 has no aspect ratio and its porosity is lower than that in Comparative Examples 1 to 2. It can be seen that the present invention affects the nucleation and growth of aragonite in the calcium carbonate cement by adding a crystal form regulator and β-cyclodextrin, thereby increasing the average aspect ratio of aragonite, reducing the porosity, forming a dense hardened structure, and enhancing the compressive strength of the hardened calcium carbonate cement. Specifically, Figure 2 The infrared images of the hardened calcium carbonate cement of Examples 1 to 4 and Comparative Examples 1 to 2 cured for 1 day show that the characteristic absorption peak of calcite appears in Comparative Example 2. This is because Comparative Example 2 has no crystal form regulator, and amorphous calcium carbonate and vaterite are transformed into calcite instead of aragonite, while Examples 1 to 4 and Comparative Example 1 add a crystal form regulator to transform into aragonite. Figure 3 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 1. Figure 4 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 2. Figure 5 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 3. Figure 6 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Example 4. Figure 7 This is the SEM image of the hardened calcium carbonate cement body cured for 1 day in Comparative Example 1. Figure 8 This is the SEM image of the hardened calcium carbonate cement of Comparative Example 2 after curing for 1 day. It can be seen from the figure that Figure 7 The aragonite structure in Figures 3 to 6 The aragonite structure is coarser, the average aspect ratio is smaller, the distribution is more uneven, and the porosity is higher, resulting in low mechanical properties; Figure 8 No crystal modifier is added, and amorphous calcium carbonate and vaterite are transformed into calcite, rather than an interdigitated needle-rod structure similar to aragonite. The calcite is rhombohedral, has no aspect ratio, and is block-stacked with large pores, resulting in low mechanical properties.
[0144] The present invention uses a crystal form regulator to regulate thermodynamically unstable amorphous calcium carbonate and vaterite to convert them into aragonite, and uses beta-cyclodextrin to modify the structure of calcium carbonate, increase the average aspect ratio of aragonite, reduce the porosity of the block, form a dense hardened structure, and significantly improve the compressive strength of the calcium carbonate cement hardened body. The calcium carbonate cement provided by the present invention has a wide range of raw materials, low cost, and is a low-carbon cement material with high strength. The hardening method is also simple and easy, so it has a wide range of applications in the field of building materials, especially the field of low-carbon building materials.
Claims
1. A calcium carbonate cement, characterized in that The invention comprises the following raw materials in parts by weight: 50 to 400 parts of amorphous calcium carbonate, 200 to 600 parts of vaterite, 10 to 600 parts of a crystal form regulator, and 10 to 800 parts of beta-cyclodextrin or its aqueous solution; the crystal form regulator comprises at least one of aragonite whiskers, coral sand or shell powder; the raw materials of the calcium carbonate cement also include water; The mass ratio of liquid to solid of the calcium carbonate cement is 0.1 to 0.
5.
2. The calcium carbonate cement according to claim 1, characterized in that The average aspect ratio of the aragonite whiskers is 5 to 40; and / or, the aragonite whiskers have an aragonite content of 85 to 100 wt %; And / or, the average particle size of the coral sand is 20 to 300 μm; And / or, the coral sand has an aragonite content of 75 to 100 wt%; And / or, the average particle size of the shell powder is 25 to 300 μm; And / or, the aragonite content of the shell powder is 70-100wt%.
3. The hardening method of calcium carbonate cement according to claim 1 or 2, characterized in that: The following steps are involved: The raw materials are mixed, molded and cured to obtain the hardened body of the calcium carbonate cement.
4. The hardening method according to claim 3, characterized in that: The molding pressure is 0 to 200 MPa; And / or, the curing time is 1 to 5 days; And / or, the curing temperature is 20-100°C.
5. A hardened calcium carbonate cement product obtained by the hardening method according to claim 3 or 4.
6. The hardened calcium carbonate cement body according to claim 5, characterized in that: The average aspect ratio of aragonite in the hardened calcium carbonate cement is 8 to 20; And / or, the porosity of the hardened calcium carbonate cement body is 30-40%.
7. Calcium carbonate cement, a method for hardening calcium carbonate cement or application of hardened calcium carbonate cement in the field of building materials, characterized in that: The calcium carbonate cement is the calcium carbonate cement described in claim 1 or 2; the hardening method of the calcium carbonate cement is the hardening method of the calcium carbonate cement described in claim 3 or 4; the hardened calcium carbonate cement body is the hardened calcium carbonate cement body described in claim 5 or 6.