A long-life composite gun barrel and preparation method thereof

By using a composite structure of a heat-resistant alloy lining with high Cr, Ni, Mo, W content and the outer layer of Cr-Ni-Mo-V steel in the artillery body tube, the problem of easy cracking of the chrome plating layer is solved, and the further development is achieved High ablation and wear resistance significantly extends the service life and stability of the artillery barrel.

CN116240428BActive Publication Date: 2024-11-22INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111491669.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-08
Publication Date
2024-11-22
Estimated Expiration
2041-12-08

AI Technical Summary

Technical Problem

During the launch process, the internal chamber cracks, cracks and peels due to ablation and wear, resulting in limited service life. The existing chrome life extension technology has internal stress and brittleness problems, making it difficult to significantly improve the life.

Method used

High temperature ablation and wear resistance alloy with high Cr, Ni, Mo and W contents are used as the inner lining, combined with the outer layer of Cr-Ni-Mo-V steel, and mechanical nesting composite is achieved through vacuum packaging welding and hot extrusion forming. , forming a composite artillery body tube that combines metallurgy.

Benefits of technology

It significantly improves the service life and quality stability of the artillery barrel, avoids cracking and peeling problems of the chrome plating layer, and improves the resistance to high-temperature ablation, wear and creep resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003399608700000051
    Figure BDA0003399608700000051
  • Figure BDA0003399608700000052
    Figure BDA0003399608700000052
  • Figure HDA0003399608710000011
    Figure HDA0003399608710000011
Patent Text Reader

Abstract

The present invention relates to the field of artillery barrel preparation technology, specifically to a long-life composite artillery barrel and a preparation method thereof. The long-life composite artillery barrel is composed of an ablation-resistant high-strength heat-resistant alloy lining and an outer layer of gun steel tube body. A heat-resistant alloy with high Cr, Ni, Mo, and W content that is resistant to high-temperature ablation and wear is selected as the lining of the outer layer of gun steel tube body. The outer layer of gun steel tube body adopts Cr-Ni-Mo-V series steel. The mechanical nesting and compounding of the heat-resistant alloy lining and the outer layer of gun steel tube body are realized by vacuum packaging welding, and the metallurgical bonding of the composite interface is realized by hot extrusion forming, and then the heat treatment of "solution aging first + quenching and tempering later" is performed to achieve the strength matching of the heat-resistant alloy lining and the outer layer of gun steel. The present invention prepares a composite artillery barrel by compositely constructing a heat-resistant alloy and gun steel. The composite artillery barrel finally obtained has excellent stiffness, high-temperature ablation resistance, wear resistance and creep resistance, and can greatly improve the service life of the artillery barrel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of gun barrel preparation technology, in particular to a long-life composite gun barrel and a preparation method thereof. Background Art

[0002] With the progress of national defense modernization, it is extremely important to improve the technical level of weapons and equipment. As an important conventional weapon, artillery has an irreplaceable position in the modern battlefield. Therefore, manufacturing high-precision and long-life artillery has become the focus of the entire weapon field. The barrel is the core component of the artillery. During the firing process of the artillery, the explosion of gunpowder produces high-temperature and high-pressure gas, which makes the inner bore of the barrel in a complex state of high temperature, high pressure, and transient high-speed impact and wear, which seriously damages the inner bore of the barrel. After repeated firing, the inner bore of the barrel cracks, cracks and falls off, which seriously affects the shooting accuracy and service life of the artillery. Modern warfare requires artillery to develop in the direction of greater power, greater rate of fire, and shorter firing intervals. Under such working conditions, the barrel will face more serious ablation, wear and fatigue problems, greatly reducing its ability to continue combat. Therefore, in the development of a new generation of artillery, the life extension technology of the barrel is particularly important.

[0003] In order to alleviate the adverse effects of ablation and wear on the inner bore of the barrel, researchers have sought various methods to improve the performance of the inner wall of the barrel. At present, the inner bore coating technology of the barrel is the main means to improve the ablation resistance of the barrel, among which electroplating chromium is the most widely used and relatively mature method to extend the life of the barrel. Due to the high wear resistance and ablation resistance of chromium, the service life of the barrel can be improved to a certain extent by electroplating chromium. However, there are always many disadvantages that are difficult to solve in the chromium plating of the barrel: 1) Due to the difference in linear expansion coefficients, the chromium layer and the gun steel layer are difficult to coordinate deformation under the action of reciprocating thermal cycles, resulting in high internal stress in the chromium layer. When it reaches a certain value, inherent cracks are formed and gradually expand during the firing process, becoming the main cause of failure. 2) Chromium has a ductile-brittle transition temperature higher than room temperature, has inherent brittleness, and its shear strength and tensile strength are both low. During the cyclic heating and cooling process of the artillery firing, the chromium plating layer is very easy to be damaged and peeled off. Due to the inherent defects of the chrome-plating technology on the inner bore of the barrel, the improvement in the barrel life is extremely limited. Therefore, there is an urgent need for more complete artillery barrel preparation technology to significantly improve the service life and quality stability of the barrel. Summary of the invention

[0004] The purpose of the present invention is to provide a long-life composite artillery barrel and a preparation method thereof, so as to solve the current problems of ablation and wear of the inner bore of the barrel due to the easy cracking, crazing and peeling of the chrome plating layer. This method can greatly improve the service life and quality stability of the artillery barrel.

[0005] The technical solution of the present invention is:

[0006] A long-life composite gun barrel consists of an ablation-resistant high-strength heat-resistant alloy lining and an outer gun steel tube body. A high-temperature ablation-resistant and wear-resistant heat-resistant alloy with high Cr, Ni, Mo, and W content is selected as the lining of the outer gun steel tube body. The outer gun steel tube body adopts Cr-Ni-Mo-V series steel. Vacuum packaging welding is used to achieve mechanical nesting and composite of the heat-resistant alloy lining and the outer gun steel tube body, and hot extrusion forming is used to achieve metallurgical bonding of the composite interface.

[0007] The long-life composite gun barrel, the composite gun barrel lining is made of a heat-resistant alloy resistant to high-temperature ablation and wear, the composition characteristics are high Cr content, and Mo and W elements are added; the specific composition range of the heat-resistant alloy lining is as follows, measured by weight percentage: C≤0.1%, Cr18.0~30.0%, Co5~9.5%, W 5~8%, Mo3~6.5%, Al 2~4.5%, Ti1~1.5%, Fe≤3%, Nb≤1.5%, Ce≤0.02%, B≤0.005%, Mn≤0.3%, Si≤0.3%, Ni balance.

[0008] The long-life composite gun barrel has an outer layer of gun steel tube body made of medium carbon Cr-Ni-Mo-V steel, and its composition range is as follows by weight percentage: C 0.2-0.4%, Cr 0.5-1.0%, Ni 2.0-4.0%, Mo 0.15-0.45%, V 0.1-0.4%, and Fe balance.

[0009] The method for preparing the long-life composite gun barrel comprises the following steps:

[0010] 1) preparing heat-resistant alloy ingots and gun steel ingots by vacuum induction melting furnace, and performing forging, punching and rolling respectively to obtain initial heat-resistant alloy tube blanks and initial gun steel tube blanks of set sizes;

[0011] 2) The outer surface of the initial heat-resistant alloy tube blank and the inner surface of the initial gun steel tube blank are milled and cleaned to ensure the inner and outer diameter dimensional accuracy of the initial heat-resistant alloy tube blank and the initial gun steel tube blank and the flush and smooth end faces of both ends to obtain the constructed heat-resistant alloy tube blank and the constructed gun steel tube blank;

[0012] 3) The heat-resistant alloy tube billet and the gun steel tube billet are fully nested and assembled to form a composite billet, ensuring that the end faces at both ends are flush, and the nested interfaces at both ends are encapsulated and welded by a vacuum electron beam welder to form a composite tube billet, ensuring that the composite interface is always in a vacuum state;

[0013] 4) The composite tube billet is heated to 1050°C ± 50°C by induction heating and kept warm for 3t / 100h, where t is the wall thickness of the composite tube billet in mm;

[0014] 5) Hot extrusion deformation connection is performed on the composite tube billet to achieve effective metallurgical bonding of the heat-resistant alloy and the gun steel interface, and an extruded composite tube billet with a heat-resistant alloy lining having a thickness of 5 to 20 mm is obtained by controlling the extrusion process;

[0015] 6) The extruded composite tube blank is subjected to a "solution aging first + quenching and tempering later" heat treatment to obtain a composite gun barrel with a heat-resistant alloy lining and an outer gun steel tube body with matching strength and toughness.

[0016] In the method for preparing the long-life composite gun barrel, in step 2), the surface roughness after milling is lower than Ra 0.8 μm.

[0017] In the method for preparing the long-life composite artillery barrel, in step 3), before nesting and assembly, alcohol or acetone is used to clean the surfaces of the heat-resistant alloy tube blank and the gun steel tube blank to be connected to avoid oil stains and foreign matter remaining on the composite interface.

[0018] The method for preparing the long-life composite gun barrel, in step 3), when the nested interfaces at both ends are packaged and welded by a vacuum electron beam welder, the nested assembled composite construction blank is placed in a vacuum chamber and evacuated to a temperature of not less than 10 - 2 Pa, the package welding depth is 5 to 50 mm.

[0019] In the method for preparing the long-life composite gun barrel, in step 5), the deformation rate of hot extrusion is 10 to 45 mm / s.

[0020] In the preparation method of the long-life composite artillery barrel, in step 6), the heat treatment process is as follows: first, the extruded composite tube blank is kept at 1000-1100°C for 1-3 hours for solution treatment, then kept at 700-800°C for 12-24 hours for aging treatment, then kept at 800-900°C for 10-30 minutes for oil quenching, and kept at 600-700°C for 1-3 hours for air cooling and tempering.

[0021] The scientific mechanism of the present invention is as follows:

[0022] 1. The selected heat-resistant alloy has excellent high-temperature strength, high-temperature ablation resistance and wear resistance. For the high-temperature strength of the alloy, firstly, a large amount of W, Mo, and Co are added for solid solution strengthening. The solute atoms can distort the lattice and form a long-range stress field; the addition of high-melting-point elements such as Mo and W can increase the interatomic bonding force and reduce the diffusion coefficient; the grain boundary strengthening elements B and Ce are added to strengthen the grain boundaries. B will produce a strong segregation phenomenon on the grain boundaries and vacancy defects, resulting in an increase in the bonding force between the grain boundaries, thereby improving the long-term creep performance of the high-temperature alloy; adding elements such as Al, Ti, and Nb to form a stable γ' precipitation strengthening phase can further strengthen the alloy. For the high-temperature ablation oxidation resistance of the alloy, adding a large amount of Cr and Al can significantly improve the oxidation resistance of the alloy. High Cr and Al content can form Cr2O3 and dense Al2O3 protective layers on the alloy surface, improving the ablation resistance of the alloy. Regarding the wear resistance of the alloy, first of all, the alloy has extremely high high temperature strength and hardness, so it has good high temperature wear resistance; in addition, the alloy has excellent high temperature strength and toughness and plasticity, which can reduce the formation and peeling of lining cracks during friction and wear; good organizational stability can avoid stress cracking and peeling during hot and cold cycle phase transformation; a large amount of γ' precipitation strengthening phase improves wear resistance.

[0023] 2. The essence of heat-resistant alloy and gun steel composite is solid-state connection, and the key lies in interface bonding. Under vacuum, high temperature, high pressure and large deformation conditions, the solid metal with a fully clean surface is close to the range of atomic force, forming a strong metal bond, and a small amount of residual microscopic holes and oxides gradually disappear under the action of diffusion, so that the interface achieves a metallurgical connection that is completely consistent with the matrix in composition, organization and performance.

[0024] 3. The construction and composite of heat-resistant alloy and gun steel involves the solid-state connection of dissimilar materials. Heat-resistant alloy and gun steel have good deformation coordination in the high temperature range of 1050℃. The two materials contain similar components and have good interface compatibility. The heterogeneous interface can be easily combined to obtain good bonding strength.

[0025] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0026] 1. In the existing artillery barrel life extension technology, a chrome-plated treatment method is often used for the inner bore of the barrel. However, due to the difference in linear expansion coefficients between the chrome-plated layer and the gun steel, there is a high internal stress at the interface during repeated thermal cycles, and chromium has natural brittleness. Therefore, the inner bore chrome-plated layer often cracks, cracks and peels off during artillery firing, which limits the service life of the artillery barrel and has extremely high quality instability. The present invention uses a composite construction method to prepare a composite artillery barrel with a certain thickness of ablation-resistant lining, which can greatly improve the service life of the artillery barrel.

[0027] 2. The present invention prepares a composite artillery barrel by composite construction of heat-resistant alloy and gun steel. Compared with chrome plating to extend life, the composite construction is achieved by hot extrusion. The process is relatively mature and will not cause a significant increase in manufacturing costs. It is practical and economical. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Schematic diagram of the forming and preparation process of heat-resistant alloy and gun steel composite pipe.

[0029] Figure 2 This is a cross-sectional view of a finished product of a heat-resistant alloy and gun steel composite pipe. In the figure, 1 is a gun steel pipe body, and 2 is a heat-resistant alloy lining.

[0030] Figure 3 Composite interface microstructure diagram. DETAILED DESCRIPTION

[0031] In the specific implementation process, the present invention proposes a long-life composite gun barrel and a preparation method thereof: first, the outer surface of the heat-resistant alloy lining and the inner surface of the outer gun steel tube body are processed and cleaned and mechanically nested together; then the assembled interface is evacuated, and the nested interface is welded by vacuum electron beam packaging to ensure that the nested interface is always in a vacuum state. The assembled nested composite tube is heated to 1050°C by induction heating and kept warm for a sufficient time, and then hot extrusion is performed to obtain a composite gun barrel with a certain lining thickness. During the high-temperature hot extrusion process, the nested interface can achieve good metallurgical bonding and have sufficient interface strength. A suitable composite heat treatment system is used to achieve the strength and toughness matching of the gun steel outer layer and the heat-resistant alloy lining. The composite gun barrel finally obtained has excellent stiffness, high-temperature ablation resistance, wear resistance and creep resistance, which can greatly improve the service life of the gun barrel.

[0032] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0033] Example 1

[0034] like Figure 1 As shown, for the construction, forming and preparation of a long-life composite artillery barrel, the specific implementation steps are as follows:

[0035] (1) High-quality heat-resistant alloy ingots and gun steel ingots are prepared by vacuum induction melting, and then forged, punched and rolled to obtain initial heat-resistant alloy tube billets and initial gun steel tube billets, see Figure 1 (a). The initial heat-resistant alloy tube size is 146 mm (outer diameter) / 98 mm (inner diameter), and the length is 1242 mm; the initial gun steel tube size is 430 mm (outer diameter) / 138 mm (inner diameter), and the length is 1243 mm.

[0036] The heat-resistant alloy lining is a heat-resistant alloy that is resistant to high-temperature ablation and wear. Its composition is required to have high Cr, Ni, Mo, and W content to ensure that it can withstand high-temperature ablation and oxidation above 1000°C, can be used for a long time above 1000°C, and has excellent room temperature and high temperature strength. The specific components of this embodiment are as follows by weight percentage:

[0037]

[0038] Regarding the selection of materials for the outer layer of gun steel pipe body, the specific components of this embodiment are as follows by weight percentage:

[0039]

[0040] (2) The initial heat-resistant alloy tube blank and the initial gun steel tube blank are milled and ground to ensure that the outer surface of the heat-resistant alloy tube blank and the inner surface of the gun steel tube blank are smooth and straight, the surface roughness reaches Ra0.1-0.2 μm, and the end faces at both ends are flush, so as to obtain the constructed heat-resistant alloy tube blank and the constructed gun steel tube blank. Figure 1 (b). The dimensions of the heat-resistant alloy tube billet are: Ф141.8mm (outer diameter) / Ф102mm (inner diameter), length 1240mm; the dimensions of the gun steel tube billet are: Ф422mm (outer diameter) / Ф142.2mm (inner diameter), length 1240mm.

[0041] (3) Use alcohol or acetone to clean the surfaces of the heat-resistant alloy tube and the gun steel tube to be connected to avoid oil stains and foreign matter remaining on the composite interface. Then, fully nest the heat-resistant alloy tube and the gun steel tube to form a composite blank, and place the nested composite blank in a vacuum chamber and evacuate to 10 -3 Pa, then the composite interface of the composite structure blank is encapsulated and welded by a vacuum electron beam welder to form a composite tube blank, and the encapsulation welding depth is about 10 to 40 mm. Figure 1 (c).

[0042] (4) The composite tube was then heated to 1050°C by induction heating and kept at this temperature for 5 hours. Figure 1 (d).

[0043] (5) The composite tube billet is subjected to hot extrusion deformation connection to achieve effective metallurgical bonding between the heat-resistant alloy and the gun steel interface. By controlling the extrusion process, an extruded composite tube billet with a heat-resistant alloy lining of a certain thickness is obtained. Figure 1 (e) and Figure 1 (f) During the hot extrusion process, the deformation rate is controlled at 25 mm / s to prevent overheating.

[0044] (6) The extruded composite tube billet is solution treated at 1080°C for 2 h, then aged at 760°C for 14-18 h, oil quenched at 850°C for 20 min, and air-cooled at 650°C for 2 h to obtain a composite gun barrel billet consisting of a heat-resistant alloy lining and an outer gun steel tube body, achieving strength and toughness matching between the heat-resistant alloy lining and the outer gun steel tube body, so that the heat-resistant alloy lining has both ablation resistance and wear resistance.

[0045] (7) The finished dimensions of the composite gun barrel obtained after machining are: Ф201mm (outer diameter) / Ф91mm (inner diameter), the wall thickness of the heat-resistant alloy lining is 5mm, and the wall thickness of the gun steel tube body is 50mm.

[0046] like Figure 2 As shown, the long-life composite artillery barrel is composed of an ablation-resistant high-strength and heat-resistant alloy lining 2 and an outer gun steel tube body 1. The heat-resistant alloy lining 2 is made of an ablation-resistant high-strength and heat-resistant alloy with high Cr and Ni content, and contains a large amount of high-melting-point elements such as Mo and W. The outer gun steel tube body 1 is made of Cr-Ni-Mo-V steel.

[0047] like Figure 3 As shown in the composite interface microstructure diagram, it can be seen that the heat-resistant alloy and the outer layer of gun steel achieve complete metallurgical bonding, there are no microscopic defects and carbide precipitation at the interface, and the composite interface has sufficient interface bonding strength.

[0048] The results of the examples show that during the firing of gunpowder, the gun barrel is subjected to high temperature, high pressure, impact and friction, resulting in severe ablation and wear. At present, chrome plating technology for the inner bore of the barrel is the main way to improve the ablation resistance of the barrel. However, due to the natural brittleness of chromium, the chrome plating layer is very prone to cracking and peeling during the hot and cold cycle, making it difficult to significantly extend the life of the gun barrel. The present invention prepares a composite gun barrel by compositely constructing ablation-resistant and wear-resistant heat-resistant alloy and gun steel. The composite gun barrel has a certain thickness of ablation-resistant and wear-resistant lining, which can withstand high-temperature ablation and wear, and significantly improves the service life and quality reliability of the gun barrel.

Claims

1. A long-life composite gun barrel, characterized in that: The long-life composite gun barrel is composed of an ablation-resistant high-strength heat-resistant alloy lining and an outer gun steel tube body. The mechanical nesting and compounding of the heat-resistant alloy lining and the outer gun steel tube body are achieved by vacuum packaging welding, and the metallurgical bonding of the composite interface is achieved by hot extrusion forming. The extruded composite tube billet is subjected to a "solution aging first + quenching and tempering later" heat treatment to obtain a composite gun barrel with a heat-resistant alloy lining and an outer gun steel tube body with matching strength and toughness. The heat treatment process is as follows: first, the extruded composite tube billet is subjected to a solution treatment at 1000-1100°C for 1-3 hours, then subjected to an aging treatment at 700-800°C for 12-24 hours, then subjected to an oil quenching at 800-900°C for 10-30 minutes, and then subjected to air cooling and tempering at 600-700°C for 1-3 hours. The specific composition range of the heat-resistant alloy lining is as follows by weight percentage: C ≤ 0.1%, Cr 18.0 ~ 30.0%, Co 5 ~ 9.5%, W 5 ~ 8%, Mo 3 ~ 6.5%, Al 2 ~ 4.5%, Ti 1 ~ 1.5%, Fe ≤ 3%, Nb ≤ 1.5%, Ce ≤ 0.02%, B ≤ 0.005%, Mn ≤ 0.3%, Si ≤ 0.3%, Ni balance; The outer gun steel tube body is a medium carbon Cr-Ni-Mo-V steel, and its composition range by weight percentage is as follows: C0.2~0.4%, Cr 0.5~1.0%, Ni 2.0~4.0%, Mo 0.15~0.45%, V 0.1~0.4%, Fe balance.

2. A method for preparing the long-life composite gun barrel according to claim 1, characterized in that: The steps include: 1) Prepare heat-resistant alloy ingots and gun steel ingots by vacuum induction melting furnace, forge, perforate and roll them respectively to obtain initial heat-resistant alloy tube billets and initial gun steel tube billets of set size; 2) The outer surface of the initial heat-resistant alloy tube blank and the inner surface of the initial gun steel tube blank are milled and cleaned to ensure the inner and outer diameter dimensional accuracy of the initial heat-resistant alloy tube blank and the initial gun steel tube blank and the flush and smooth end faces at both ends to obtain the constructed heat-resistant alloy tube blank and the constructed gun steel tube blank; 3) The heat-resistant alloy tube billet and the gun steel tube billet are fully nested and assembled to form a composite billet, ensuring that the end faces at both ends are flush, and the nested interfaces at both ends are encapsulated and welded by a vacuum electron beam welder to form a composite tube billet, ensuring that the composite interface is always in a vacuum state; 4) The composite tube billet is heated to 1050°C ± 50°C by induction heating and kept warm for 5 hours; 5) Hot extrusion deformation connection is performed on the composite tube billet to achieve effective metallurgical bonding of the heat-resistant alloy and the gun steel interface, and an extruded composite tube billet with a heat-resistant alloy lining having a thickness of 5 to 20 mm is obtained by controlling the extrusion process; 6) The extruded composite tube billet is subjected to a "solution aging first + quenching and tempering later" heat treatment to obtain a composite gun barrel with a heat-resistant alloy lining and an outer gun steel tube body with matching strength and toughness.

3. The method for preparing a long-life composite gun barrel according to claim 2, characterized in that: In step 2), the surface roughness after milling is less than Ra 0.8 μm.

4. The method for preparing a long-life composite gun barrel according to claim 2, characterized in that: In step 3), before nesting and assembling, use alcohol or acetone to clean the surfaces of the heat-resistant alloy tube and the gun steel tube to be connected to avoid oil stains and foreign matter remaining on the composite interface.

5. The method for preparing a long-life composite gun barrel according to claim 2, characterized in that: In step 3), when the nested interfaces at both ends are packaged and welded using a vacuum electron beam welder, the nested assembled composite structure blank is placed in a vacuum chamber and evacuated to a temperature of not less than 10 -2 Pa, the package welding depth is 5~50mm.

6. The method for preparing a long-life composite gun barrel according to claim 2, characterized in that: In step 5), the deformation rate of hot extrusion is 10~45mm / s.

7. The method for preparing a long-life composite gun barrel according to claim 2, characterized in that: In step 6), the heat treatment process is as follows: first, the extruded composite tube is subjected to a solution treatment at 1000-1100°C for 1-3 hours, then subjected to an aging treatment at 700-800°C for 12-24 hours, then subjected to oil quenching at 800-900°C for 10-30 minutes, and then subjected to air cooling and tempering at 600-700°C for 1-3 hours.