Non-quenched and tempered weathering steel, preparation method and fastener
By adding specific elements to weathering steel and adopting smelting and temperature-controlled rolling technology, a high-strength, high-weather-resistant non-temperature weathering steel is prepared, which solves the problem of insufficient strength of weathering steel and achieves high yield and tensile strength and provide good performance support for fasteners.
Patent Information
- Application Number
- CN202211606530.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-12
AI Technical Summary
The existing weather-resistant steels corrode and age quickly in outdoor environments, which affects the service life and safety of buildings. They have low strength and yield strength less than 400MPa, making it difficult to meet application needs.
The non-temperature weathering steel components, including carbon, silicon, manganese, copper, chromium, nickel, titanium, boron, molybdenum, are prepared through smelting, temperature-controlled rolling, shot blasting, phosphating and saponification treatment. Weathering steel with a strength of not less than 1600MPa and a tensile strength of not less than 1700MPa, and is used for the manufacture of fasteners.
The strength and weather resistance of weathering steel are significantly improved, making its yield strength and tensile strength higher than most non-tempered steels on the market, and the fastener performance level reaches 16.9, making it suitable for outdoor use.
Smart Images

Figure CN116240454B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonferrous metal production, and in particular to non-quenched and tempered weathering steel and a preparation method and a fastener. Background Art
[0002] The heat treatment method of high temperature tempering after quenching is called tempering. Tempering can adjust the performance and material of steel to a great extent. Its strength, plasticity and toughness are better, and it has good comprehensive mechanical properties.
[0003] In outdoor building construction, the weather resistance of steel is required to be relatively high, otherwise the steel will corrode and age rapidly in the outdoor environment, which will affect the service life and safety of the building. However, the existing weathering steel generally has the problem of low strength, and its yield strength rarely exceeds 400MPa, which is quite different from quenched and tempered steel, limiting the application of weathering steel.
[0004] To temper steel, the steel needs to be placed in heat treatment equipment. For steel with large volume and length, ordinary heat treatment processes are difficult to penetrate into the interior of the steel, and the size and weight of the steel exceed the carrying capacity of the heat treatment equipment. Especially for long bars, due to the decrease in hardness during the heat treatment process, they will also bend under the action of their own gravity, making it difficult to use existing heat treatment equipment for tempering. Summary of the invention
[0005] The purpose of the present invention is to provide a non-quenched and tempered weathering steel which has the advantages of high strength and weather resistance, so as to solve the problem of poor strength of weathering steel.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A non-quenched and tempered weathering steel comprises the following components by weight: 0.25% to 0.35% carbon, 0.25% to 0.65% silicon, 1.4% to 2.5% manganese, ≤0.02% sulfur, 0.06% to 0.12% phosphorus, 0.25% to 0.5% copper, 0.61% to 1.25% chromium, 0.12% to 0.65% nickel, 0.04% to 0.1% titanium, 0.0005% to 0.0035% boron, 0.25% to 0.35% vanadium, 0.50% to 0.65% molybdenum, 0.1-0.24% nitrogen, and the balance is iron and unavoidable impurities.
[0008] Preferably, the yield strength of the non-quenched and tempered weathering steel is not less than 1600 MPa.
[0009] Preferably, the tensile strength of the non-quenched and tempered weathering steel is not less than 1700 MPa.
[0010] The present invention also provides a method for preparing any of the above non-quenched and tempered weathering steels, comprising the following steps:
[0011] S1: mixing the raw materials according to the ingredients, smelting the raw materials to obtain steel billets;
[0012] S2: rolling and cooling the steel billet to obtain non-quenched and tempered steel;
[0013] Preferably, the rolling is temperature-controlled rolling, specifically, the final rolling temperature is controlled at 770-820°C.
[0014] Preferably, the cooling rate is 3-5°C / s.
[0015] The present invention also provides a fastener made from any of the above-mentioned non-quenched and tempered weathering steels.
[0016] Preferably, the fastener preparation process includes: subjecting non-quenched and tempered weathering steel to shot blasting, phosphating, saponifying, wire drawing, and then cold forging and thread rolling to obtain the fastener.
[0017] Preferably, the fastener preparation process includes: subjecting the non-quenched and tempered weathering steel to shot blasting, phosphating, saponifying, wire drawing, hot forging, and thread rolling to obtain the fastener.
[0018] In the non-quenched and tempered weathering steel of the present invention, elements such as boron, nickel, chromium, and molybdenum can increase steel fine particles, copper and nickel can improve the strength and yield ratio of steel and significantly improve weather resistance, silicon and phosphorus can improve the strength of steel, and the combined use of phosphorus and copper can improve the fatigue resistance and weather resistance of steel, vanadium can improve the strength and yield ratio of steel, chromium can increase hardenability and has a secondary hardening effect, and manganese can improve the strength and hardenability of steel.
[0019] To sum up, due to the adoption of the above-mentioned technical scheme, the beneficial effects of the present invention are: the non-quenched and tempered weathering steel of the present invention is mainly composed of pearlite and ferrite, with a yield strength of up to 1660MPa and a tensile strength of up to 1765MPa, which are higher than the strength of most non-quenched and tempered steel products on the market, and also have good weather resistance; the fasteners manufactured using the non-quenched and tempered weathering steel have a performance grade of up to 16.9 and have good weather resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The metallographic photograph of non-quenched and tempered weathering steel prepared by the method in Example 9 using the raw materials in Example 5.
[0021] Figure 2 The metallographic photograph of non-quenched and tempered weathering steel prepared by the method in Example 10 using the raw materials in Example 4. DETAILED DESCRIPTION
[0022] The invention provides a non-quenched and tempered weathering steel, which comprises the following components by weight: 0.25% to 0.35% carbon, 0.25% to 0.65% silicon, 1.4% to 2.5% manganese, ≤0.02% sulfur, 0.06% to 0.12% phosphorus, 0.25% to 0.5% copper, 0.61% to 1.25% chromium, 0.12% to 0.65% nickel, 0.04% to 0.1% titanium, 0.0005% to 0.0035% boron, 0.25% to 0.35% vanadium, 0.50% to 0.65% molybdenum, 0.1-0.24% nitrogen, and the balance is iron and inevitable impurities.
[0023] The present invention also provides a method for preparing non-quenched and tempered weathering steel, comprising the following steps:
[0024] S1: According to the above ingredients, the raw materials are smelted, and the smelting steps include converter smelting → refining → continuous casting to obtain steel billets;
[0025] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 770-820°C, and then cooled at a cooling rate of 3-5°C / s to obtain non-quenched and tempered steel;
[0026] S3: Shot blasting, phosphating and saponifying the non-quenched and tempered steel to obtain non-quenched and tempered weathering steel.
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0028] Example 1
[0029] The present embodiment provides a non-quenched and tempered weathering steel, which comprises the following components by weight: 0.25% carbon, 0.25% silicon, 1.4% manganese, 0.017% sulfur, 0.06% phosphorus, 0.25% copper, 0.61% chromium, 0.12% nickel, 0.04% titanium, 0.0005% boron, 0.25% vanadium, 0.50% molybdenum, 0.10% nitrogen, and the balance is iron and unavoidable impurities.
[0030] Example 2
[0031] The present embodiment provides a non-quenched and tempered weathering steel, which comprises the following components by weight: 0.27% carbon, 0.35% silicon, 1.7% manganese, 0.013% sulfur, 0.08% phosphorus, 0.30% copper, 0.70% chromium, 0.20% nickel, 0.06% titanium, 0.001% boron, 0.28% vanadium, 0.55% molybdenum, 0.13% nitrogen, and the remainder is iron and unavoidable impurities.
[0032] Example 3
[0033] The present embodiment provides a non-quenched and tempered weathering steel, which comprises the following components by weight: 0.3% carbon, 0.45% silicon, 2.0% manganese, 0.015% sulfur, 0.10% phosphorus, 0.40% copper, 0.80% chromium, 0.30% nickel, 0.08% titanium, 0.015% boron, 0.30% vanadium, 0.60% molybdenum, 0.16% nitrogen, and the remainder is iron and unavoidable impurities.
[0034] Example 4
[0035] The present embodiment provides a non-quenched and tempered weathering steel, which comprises the following components by weight: 0.35% carbon, 0.55% silicon, 2.5% manganese, 0.009% sulfur, 0.12% phosphorus, 0.50% copper, 1.00% chromium, 0.45% nickel, 0.10% titanium, 0.0025% boron, 0.35% vanadium, 0.65% molybdenum, 0.20% nitrogen, and the remainder is iron and unavoidable impurities.
[0036] Example 5
[0037] The present embodiment provides a non-quenched and tempered weathering steel, which comprises the following components by weight: 0.40% carbon, 0.65% silicon, 3.0% manganese, 0.013% sulfur, 0.15% phosphorus, 0.60% copper, 1.25% chromium, 0.65% nickel, 0.12% titanium, 0.0035% boron, 0.40% vanadium, 0.70% molybdenum, 0.24% nitrogen, and the remainder is iron and unavoidable impurities.
[0038] Example 6
[0039] This embodiment provides a method for preparing non-quenched and tempered weathering steel, comprising the following steps:
[0040] S1: Mix the raw materials according to the ingredients, smelt the raw materials and make steel billets;
[0041] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 770°C, and then cooled at a cooling rate of 3°C / s to obtain non-quenched and tempered steel;
[0042] S3: Shot blasting, phosphating and saponifying the non-quenched and tempered steel to obtain non-quenched and tempered weathering steel.
[0043] Example 7
[0044] This embodiment provides a method for preparing non-quenched and tempered weathering steel, comprising the following steps:
[0045] S1: Mix the raw materials according to the ingredients, smelt the raw materials and make steel billets;
[0046] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 780°C, and then cooled at a cooling rate of 3°C / s to obtain non-quenched and tempered steel;
[0047] S3: Shot blasting, phosphating and saponifying the non-quenched and tempered steel to obtain non-quenched and tempered weathering steel.
[0048] Example 8
[0049] This embodiment provides a method for preparing non-quenched and tempered weathering steel, comprising the following steps:
[0050] S1: Mix the raw materials according to the ingredients, smelt the raw materials and make steel billets;
[0051] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 790°C, and then cooled at a cooling rate of 3.5°C / s to obtain non-quenched and tempered steel;
[0052] S3: Shot blasting, phosphating and saponifying the non-quenched and tempered steel to obtain non-quenched and tempered weathering steel.
[0053] Example 9
[0054] This embodiment provides a method for preparing non-quenched and tempered weathering steel, comprising the following steps:
[0055] S1: Mix the raw materials according to the ingredients, smelt the raw materials and make steel billets;
[0056] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 800°C, and then cooled at a cooling rate of 4.0°C / s to obtain non-quenched and tempered steel;
[0057] S3: Shot blasting, phosphating and saponifying the non-quenched and tempered steel to obtain non-quenched and tempered weathering steel.
[0058] Example 10
[0059] This embodiment provides a method for preparing non-quenched and tempered weathering steel, comprising the following steps:
[0060] S1: Mix the raw materials according to the ingredients, smelt the raw materials and make steel billets;
[0061] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 810°C, and then cooled at a cooling rate of 4.5°C / s to obtain non-quenched and tempered steel;
[0062] S3: Shot blasting, phosphating and saponifying the non-quenched and tempered steel to obtain non-quenched and tempered weathering steel.
[0063] Embodiment 11
[0064] This embodiment provides a method for preparing non-quenched and tempered weathering steel, comprising the following steps:
[0065] S1: Mix the raw materials according to the ingredients, smelt the raw materials and make steel billets;
[0066] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 820°C, and then cooled at a cooling rate of 5.0°C / s to obtain non-quenched and tempered steel;
[0067] S3: Shot blasting, phosphating and saponifying the non-quenched and tempered steel to obtain non-quenched and tempered weathering steel.
[0068] The proportions of ingredients in Examples 1-5 were used to prepare non-quenched and tempered weathering steel according to the preparation methods in Examples 6-11, and the yield strength Rm, tensile strength ReL, and weathering resistance thereof were as shown in Tables 1, 2, and 3, respectively:
[0069] Table 1 Yield strength of different non-quenched and tempered weathering steels
[0070]
[0071] As shown in Table 1 above, the yield strength of the prepared non-quenched and tempered weathering steel is higher than 1250 MPa, and the maximum yield strength can reach 1660 MPa.
[0072] Table 2 Tensile strength of different non-quenched and tempered weathering steels
[0073]
[0074] As shown in Table 2 above, the yield strength of the non-quenched and tempered weathering steels produced is higher than 1400 MPa, and the maximum yield strength can reach 1765 MPa.
[0075] According to the medium-cycle immersion corrosion test method of TB / T2375 standard, the prepared non-quenched and tempered weathering steel was tested for 100 hours. The results are shown in Table 3 below:
[0076] Table 3 Weathering resistance of different non-quenched and tempered weathering steels
[0077]
[0078] As shown in Table 1 above, the weight loss rate of the non-quenched and tempered weathering steel can be as low as 0.014 g / (m2·h).
[0079] Comparative Example 1
[0080] A non-quenched and tempered weathering steel comprises the following components by weight: 0.012% carbon, 0.15% silicon, 0.44% manganese, 0.014% phosphorus, 0.005% sulfur, 0.037% Al, 0.35% copper, 5.45% chromium, 0.31% nickel, 0.021% titanium, 0.0.003% nitrogen, 0.012% rhenium, and the balance is iron and unavoidable impurities.
[0081] The weathering steel production method of comparative example 1 is: after continuous casting of molten steel, it is subjected to hot rolling, pickling, cold rolling and continuous annealing. The yield strength is tested to be 591 MPa and the tensile strength is 431 MPa, both of which are lower than the combination of embodiments 1 to 5 and embodiments 6 to 11.
[0082] like Figure 1 , 2 ,in Figure 1 This is a metallographic photograph of non-quenched and tempered weathering steel prepared using the raw materials of Example 5 according to the method of Example 9. Figure 2 The metallographic photograph of the non-quenched and tempered weathering steel prepared by the method in Example 10 using the raw materials in Example 4. It can be seen from the image that the non-quenched and tempered weathering steel is mainly composed of pearlite ( Figure 1 , 2 Medium dark area) and ferrite ( Figure 1 , 2 The pearlite content is much higher than that of ordinary weathering steel, and they are interconnected, wrapping most of the ferrite, making the yield strength and tensile strength of the steel significantly higher than that of ordinary weathering steel.
[0083] The non-quenched and tempered weathering steels in Tables 1 to 3 have a high yield strength ratio and are suitable as raw materials for fasteners. For example, by subjecting the non-quenched and tempered weathering steel billets to shot blasting, phosphating, saponifying, wire drawing, and then cold forging and thread rolling processes, high-strength fasteners can be obtained.
[0084] Fasteners can also be prepared in another way. The specific preparation method is: the above non-quenched and tempered weathering steel is shot blasted, phosphated, saponified, and wire drawn, and then subjected to hot forging and thread rolling processes to obtain fasteners with high strength.
[0085] The fasteners obtained by the above two processes have a performance grade of up to 16.9 and have good corrosion resistance, making them suitable for use in outdoor environments.
[0086] In addition, the non-quenched and tempered weathering steels in Tables 1 to 3 can also be used to manufacture piston rods. For example, by drawing, straightening, polishing, and chrome-plating the round non-quenched and tempered weathering steel, a high-strength piston rod can be obtained.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A non-quenched and tempered weathering steel, characterized in that: Prepared as follows, S1. The following components are formulated, by weight, carbon 0.25%~0.35%, silicon 0.25%~0.65%, manganese 1.4%~2.5%, sulfur ≤0.02%, phosphorus 0.06%~0.12%, copper 0.25%~0.5%, chromium 0.61%~1.25%, nickel 0.12%~0.65%, titanium 0.04%~0.1%, boron 0.0005%~0.0035%, vanadium 0.25%~0.35%, molybdenum 0.50%~0.65%, nitrogen 0.1-0.24%, the balance is iron and unavoidable impurities, the raw materials are smelted to obtain steel billets; S2: rolling and cooling the steel billet to obtain non-quenched and tempered weathering steel, wherein the rolling is temperature-controlled rolling, the final rolling temperature is controlled at 770-820° C., and the cooling rate is 3-5° C. / s; The non-quenched and tempered weathering steel consists of pearlite and ferrite.
2. The non-quenched and tempered weathering steel according to claim 1, characterized in that: The yield strength of the non-quenched and tempered weathering steel is not less than 1600 MPa.
3. The non-quenched and tempered weathering steel according to claim 1, characterized in that: The tensile strength of the non-quenched and tempered weathering steel is not less than 1700 MPa.
4. A fastener, characterized in that: It is made using the non-quenched and tempered weathering steel as described in any one of claims 1 to 3.
5. The fastener according to claim 4, characterized in that The preparation process comprises: subjecting non-quenched and tempered weathering steel to shot blasting, phosphating, saponifying, wire drawing, cold forging and thread rolling to obtain the fastener.
6. The fastener according to claim 4, characterized in that The preparation process comprises: subjecting non-quenched and tempered weathering steel to shot blasting, phosphating, saponifying and wire drawing, and then to hot forging and thread rolling to obtain the fastener.