Iron titanate / cerium oxide composite material and preparation method thereof

By preparing the iron titanate/cerium oxide composite material, and using hydrothermal reaction and calcining steps to form a type II heterojunction structure, the gap in the preparation and application of the iron titanate/cerium oxide composite material in the prior art is solved, and high-efficiency light is achieved Catalytic activity and organic degradation effect are simple and cheap.

CN116251593BActive Publication Date: 2024-11-26NANTONG VOCATIONAL COLLEGE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310256545.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-16
Publication Date
2024-11-26
Estimated Expiration
2043-03-16

AI Technical Summary

Technical Problem

The lack of preparation and application of iron titanate/cerium oxide composites in the prior art limits its potential performance in the field of photocatalysis.

Method used

The iron titanate/cerium oxide composite material was prepared by two-step method. Through hydrothermal reaction and calcination steps, a nanocomposite material with type II heterojunction structure was formed, which optimized the generation, migration and separation of its photogenerated charges and improved photocatalytic activity. .

Benefits of technology

It realizes the efficient visible light absorption performance and excellent photocatalytic activity of the composite material, and has a good degradation effect on carbon dioxide and organic matter, with simple steps and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116251593B_ABST
    Figure CN116251593B_ABST
Patent Text Reader

Abstract

The invention discloses an iron titanate / cerium oxide composite material and a preparation method thereof. The preparation method comprises the following steps: (1) preparing nano iron titanate: adding an iron source to anhydrous ethanol, stirring until completely dissolved, then dropping a titanium source, continuously stirring and dropping ethylenediamine to form a sol, then performing a hydrothermal reaction, cooling and washing with water, washing with alcohol, vacuum drying, and calcining under inert gas protection to obtain nano iron titanate; (2) preparing an iron titanate / cerium oxide composite material: adding the nano iron titanate obtained in step (1) to anhydrous ethanol, then adding octadecylamine, polyvinyl pyrrolidone and a cerium source, stirring and then performing a hydrothermal reaction, washing and vacuum drying the obtained precipitate, and obtaining an iron titanate / cerium oxide composite material. The two-step method is used to prepare the iron titanate / cerium oxide composite material, which has simple steps and low price. Cerium oxide and iron titanate are compounded by a hydrothermal reaction, so that efficient reduction of carbon dioxide can be achieved, and at the same time, a good photodegradation effect is achieved on various organic substances.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite semiconductor photocatalytic materials, and in particular relates to an iron titanate / cerium oxide composite material and a preparation method thereof. Background Art

[0002] Water pollution caused by organic pollutants poses a serious threat to ecosystems and human health. Microbial-induced biodegradation is an inexpensive and common method for oxidizing organic pollutants in water. The treatment environment and treatment time are demanding, which to a certain extent affects the treatment efficiency of biodegradation. Physical adsorption is a simple treatment method that is often used as an alternative to biodegradation. However, physical adsorption requires tedious post-treatment of the adsorbate and the used adsorbent. Due to the shortcomings of traditional water treatment methods, researchers have been committed to developing more efficient and environmentally friendly water treatment methods to degrade organic pollutants in water. The photo-Fenton reaction is an advanced oxidation reaction that is a clean and effective method for generating active substances with excellent oxidation ability to remove various organic pollutants. In the search for new photo-Fenton catalysts, people have paid considerable attention to the abundant and non-toxic iron-based heterogeneous structures as promising catalytic systems for the removal of organic pollutants. Wang Xuejiang's team from Tongji University (10.1016 / j.jhazmat.2021.127387) used a simple impregnation calcination method to convert FeMo3O x and g-C3N4 were grown in situ onto the surface of perlite to prepare a photo-Fenton hybrid catalytic system, which showed excellent removal efficiency for tetracycline, oxytetracycline and chlortetracycline through the photo-Fenton reaction. The team of Lai Cui from Hunan University (10.1016 / j.jcis.2021.10.033) synthesized a flower-like MnFe2O4 / MoS2 hybrid system and used it to degrade tetracycline in contaminated water through an efficient photo-Fenton reaction.

[0003] Iron titanate is a type of perovskite titanate material and also a semiconductor material. It has attracted attention because of its unique magnetic and electrical properties. Recent studies have found that iron titanate has certain photocatalytic activity. For example, Ramezani et al. (10.1007 / s10854-015-2930-6) found that iron titanate exhibited good photocatalytic activity in the field of photocatalysis. For the first time, oxalic acid was used as a chelating agent to synthesize iron titanate nanoparticles by sol-gel method. The effects of different surfactants such as oleic acid, oleylamine, sodium dodecyl sulfate and hexadecyltrimethylammonium bromide on the particle size of the final product were studied. The synthesized photocatalyst was used for the decolorization of rhodamine B (RhB) and methylene blue (MB) to study its light harvesting application. The photocatalyst results showed that under ultraviolet light irradiation, the maximum decolorization rates of iron titanate nanoparticle catalysts for rhodamine B and methylene blue were 93% and 95% respectively within a reaction time of 40 minutes. Feng Shouhua's team from Jilin University (10.1039 / C8NR01331D) modified the surface of pure iron titanate with fluorine. The synergistic effect of nanostructure and surface fluorine modification gave it higher solar water splitting performance.

[0004] Chinese patent CN202011316229.8 A preparation method and application of iron titanate nanomaterials. This preparation method uses pre-lithiated iron titanate as the negative electrode active material of the lithium-ion hybrid supercapacitor. The disclosed preparation method is simple, has no pollution before and after the reaction, and has relatively low cost.

[0005] However, to date, there has been no report on the preparation and application of iron titanate / cerium oxide composites.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing an iron titanate / cerium oxide composite material, which has simple steps and low cost. The prepared composite material is a type II heterojunction, which is conducive to the generation, migration and separation of photogenerated charges, prolongs the life of photogenerated charges, effectively improves its absorption performance of visible light, and thus improves the photocatalytic activity.

[0008] The present invention also aims to provide an iron titanate / cerium oxide composite material.

[0009] To achieve the above object, the present invention provides a method for preparing an iron titanate / cerium oxide composite material, comprising the following steps:

[0010] (1) Preparation of nano iron titanate: adding an iron source to anhydrous ethanol, stirring until completely dissolved, then adding a titanium source dropwise, adding ethylenediamine dropwise under continuous stirring to form a sol, and then performing a hydrothermal reaction, cooling, washing with water, washing with alcohol, vacuum drying, and calcining under inert gas protection to obtain nano iron titanate;

[0011] (2) Preparation of iron titanate / cerium oxide composite material: The nano iron titanate obtained in step (1) is added to anhydrous ethanol, and then octadecylamine, polyvinyl pyrrolidone and a cerium source are added, and the mixture is stirred and subjected to a hydrothermal reaction. The obtained precipitate is washed and vacuum dried to obtain an iron titanate / cerium oxide composite material.

[0012] In the present invention, the hydrothermal reaction and calcination operations are both carried out in equipment commonly used in the art, and the present application does not make any special limitation. For example, the hydrothermal reaction is carried out in a hydrothermal kettle, and the calcination is carried out in a tubular furnace.

[0013] In the preparation method of the iron titanate / cerium oxide composite material described in the present invention, in step (1), the iron in the iron source is a positive trivalent ion, and the molar ratio of the iron element in the iron source to the titanium element in the titanium source is 1:1; the amount of ethylenediamine added is based on the observation that the solution forms a sol.

[0014] In the method for preparing the iron titanate / cerium oxide composite material of the present invention, in step (1), the iron source is one or more of ferric nitrate, ferric chloride and ferric sulfate.

[0015] In the method for preparing the iron titanate / cerium oxide composite material of the present invention, in step (1), the titanium source is tetrabutyl titanate and / or tetraisopropyl titanate.

[0016] In the preparation method of the iron titanate / cerium oxide composite material of the present invention, in step (1), the hydrothermal reaction conditions are: temperature of 160-200° C., and reaction time of 8-24 hours.

[0017] In the preparation method of the iron titanate / cerium oxide composite material of the present invention, in step (1), the calcination conditions are: temperature of 650-700° C. and time of 2-3 hours.

[0018] In the preparation method of the iron titanate / cerium oxide composite material described in the present invention, in step (2), the molar ratio of the iron element in the iron titanate to the cerium element in the cerium source is 1 to 2:2; the mass ratio of octadecylamine to the cerium source is 1 to 2:10; and the mass ratio of polyvinyl pyrrolidone to the cerium source is 1 to 2:2.

[0019] In the method for preparing the iron titanate / cerium oxide composite material of the present invention, in step (2), the hydrothermal reaction conditions are: temperature of 160-200° C., and reaction time of 80-120 minutes.

[0020] To achieve the above object, the present invention also provides an iron titanate / cerium oxide composite material prepared by the above-mentioned preparation method.

[0021] Beneficial effects of the present invention:

[0022] The iron titanate / cerium oxide composite material is prepared by a two-step method, which has simple preparation steps and low raw material prices. Cerium oxide and iron titanate are compounded by hydrothermal reaction, and the obtained composite material has a typical type II heterojunction structure, constructs a three-dimensional electric field space, and is conducive to the efficient migration and separation of photogenerated electrons and holes, so that the composite material has excellent visible light catalytic performance, can achieve efficient reduction of carbon dioxide, and has a good photodegradation effect on various organic matter. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the XRD diagram of the sample obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0025] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0026] The reagents and raw materials used in the present invention are shown in Table 1 below:

[0027] Table 1 Reagents and raw materials used in the present invention

[0028]

[0029] Example 1

[0030] Accurately weigh 3.56 grams of iron nitrate and dissolve it in 50 milliliters of anhydrous ethanol to form a reddish brown solution. Use a pipette to accurately pipette 3 milliliters of tetrabutyl titanate (about 3 grams) and add it dropwise to the above solution while stirring. After continuing to stir for 30 minutes, transfer the solution to a 100-ml hydrothermal kettle, drop ethylenediamine until the solution forms a sol, add anhydrous ethanol to about 70%, and react at 200°C for 12 hours. The obtained precipitate is washed with water and alcohol and then vacuum dried at 60°C. The product is calcined at 700°C in a tubular furnace under nitrogen protection for 2 hours to obtain iron titanate. Accurately weigh 0.5 g of the above-mentioned iron titanate, add it to 50 ml of anhydrous ethanol, add 1.26 g of cerium nitrate, 0.126 g of octadecylamine, and 1.26 g of polyvinyl pyrrolidone, stir for 30 minutes, transfer it to a 100 ml hydrothermal kettle, and perform hydrothermal reaction at 180°C for 100 minutes. The obtained precipitate is washed and vacuum dried to obtain an iron titanate / cerium oxide composite material.

[0031] The iron titanate / cerium oxide composite material prepared in Example 1 of the present invention was subjected to XRD analysis using a D8 Advance X-ray diffractometer from Bruker Spectroscopy Instruments of Germany. The results are as follows: Figure 1 As shown, the test conditions are: Cu target Kα line, λ=0.15406nm, 2θ is 10°~70°, and the scanning speed is 5(°) / min. Figure 1 The strong diffraction peaks at 28.5°, 33.0°, 47.4°, 56.4°, 59.1° and 69.5° correspond to the (111), (200), (220), (311), (222) and (400) crystal planes of face-centered cubic fluorite structure cerium dioxide (PDF card 75-0390), space group Fm-3m, a=b=c=5.411. The remaining diffraction peaks are all attributed to the (002), (200), (201), (110), (111), (112), (203), (004), (310), (400) and (113) crystal planes of iron titanate (PDF card 73-1631) with Ccmm space group. All the fronts are sharp, indicating that the prepared samples have good crystal form and high purity.

[0032] 50 mg of the prepared iron titanate / cerium oxide composite material and 100 ml of ultrapure water were added to a 250 ml photoreactor with an optical quartz window on the top of the reactor, and then the mixture was ultrasonically treated for 10 minutes to obtain a suspension. A 300-watt xenon lamp with a filter (λ>400 nm) was used as the light source. Before illumination, the reactor was evacuated and then purged with ultrapure carbon dioxide (99.99%) for 1 hour to achieve saturated dissolution and adsorption / desorption equilibrium of the suspension for carbon dioxide. The pressure in the reactor was 100 kPa, and the circulating water temperature was controlled to be maintained at 25°C. During the reaction, the gas mixture was sampled from the reaction cell every 1 hour and analyzed by a gas chromatograph equipped with a thermal conductivity detector using argon as the carrier gas. At the same reaction time interval, 0.5 ml of the liquid product was extracted from the reactor and mixed with 0.1 ml of D2O, and 1.67 ppm of dimethyl sulfoxide was added as a standard. Measured using a 400 MHz nuclear magnetic resonance spectrometer 1 H NMR spectrum is used to analyze the liquid phase products and content in the photocatalytic reduction of carbon dioxide. According to the test, the selectivity and yield of the product carbon monoxide are 86.4% and 9.23 mmol / g / h respectively.

[0033] Example 2

[0034] Accurately weigh 3.56 grams of iron nitrate and dissolve it in 50 milliliters of anhydrous ethanol to form a reddish brown solution. Use a pipette to accurately pipette 3 milliliters of tetrabutyl titanate (about 3 grams) and add it dropwise to the above solution while stirring. After continuing to stir for 30 minutes, transfer the solution to a 100-ml hydrothermal kettle, drop ethylenediamine until the solution forms a sol, add anhydrous ethanol to about 70%, and react at 160°C for 24 hours. The obtained precipitate is washed with water and alcohol and then vacuum dried at 60°C. The product is calcined at 650°C in a tubular furnace under nitrogen protection for 3 hours to obtain iron titanate. Accurately weigh 0.8 g of the above-mentioned iron titanate, add it to 50 ml of anhydrous ethanol, add 1.26 g of cerium nitrate, 0.19 g of octadecylamine, and 0.8 g of polyvinyl pyrrolidone, stir for 30 minutes, transfer it to a 100 ml hydrothermal kettle, and carry out hydrothermal reaction at 160°C for 120 minutes. The obtained precipitate is washed and vacuum dried to obtain an iron titanate / cerium oxide composite material.

[0035] 0.4 g of the prepared iron titanate / cerium oxide composite material was placed in a beaker containing 100 ml of a 10 mg / L phenol solution, subjected to ultrasonic treatment for 2 minutes, dark adsorbed for 30 minutes, and then illuminated for 30 minutes with a 300-W xenon lamp at a distance of 20 cm from the liquid surface under stirring. The degraded solution was centrifuged and its absorbance at 269 nm was measured by a UV-visible spectrophotometer. The degradation rate of phenol was calculated to be 87.8%.

[0036] Example 3

[0037] Accurately weigh 3 grams of ferric nitrate and dissolve it in 50 milliliters of anhydrous ethanol to form a reddish brown solution. Use a pipette to accurately pipette 2.5 milliliters of tetrabutyl titanate (about 2.5 grams) and add it dropwise to the above solution while stirring. After continuing to stir for 30 minutes, transfer the solution to a 100 milliliter hydrothermal kettle, drop ethylenediamine until the solution forms a sol, add anhydrous ethanol to about 70%, and react at 200°C for 8 hours. The obtained precipitate is washed with water and alcohol and then vacuum dried at 60°C. The product is calcined at 700°C in a tubular furnace under nitrogen protection for 2 hours to obtain ferric titanate. Accurately weigh 0.8 g of the above-mentioned iron titanate, add it to 50 ml of anhydrous ethanol, add 1.26 g of cerium nitrate, 0.252 g of octadecylamine, and 0.63 g of polyvinyl pyrrolidone, stir for 30 minutes, transfer it to a 100 ml hydrothermal kettle, and perform hydrothermal reaction at 200°C for 80 minutes. The obtained precipitate is washed and vacuum dried to obtain an iron titanate / cerium oxide composite material.

[0038] 0.6 g of the prepared iron titanate / cerium oxide composite material was taken and placed in a beaker containing 100 ml of a 10 mg / L tetracycline solution. After ultrasonic treatment for 2 minutes and dark adsorption for 30 minutes, it was illuminated for 60 minutes with a 300-watt xenon lamp light source at a distance of 20 cm from the liquid surface under stirring. After centrifugation, the solution after degradation was measured by a UV-visible spectrophotometer for its absorbance at 357 nm. The degradation rate of tetracycline was calculated to be 96.8%.

[0039] Comparative Example 1

[0040] 1.26 g of cerium nitrate, 0.126 g of octadecylamine, and 0.63 g of polyvinyl pyrrolidone were accurately weighed, stirred for 30 minutes, and then transferred into a 100 ml hydrothermal kettle for hydrothermal reaction at 200°C for 80 minutes. The obtained precipitate was washed and vacuum dried to obtain cerium oxide. 0.5 g of the cerium oxide and 0.5 g of the iron titanate prepared in Example 3 were weighed, put into a mortar, and ground thoroughly to obtain a physically mixed iron titanate / cerium oxide composite material.

[0041] 0.6 g of the physically mixed iron titanate / cerium oxide composite material prepared above was taken and placed in a beaker containing 100 ml of a 10 mg / L tetracycline solution. After ultrasonic treatment for 2 minutes and dark adsorption for 30 minutes, the solution was illuminated for 60 minutes at a distance of 20 cm from the liquid surface by a 300-W xenon lamp light source under stirring. After centrifugation, the solution after degradation was measured by a UV-visible spectrophotometer for its absorbance at 357 nm. The degradation rate of tetracycline was calculated to be 52.4%.

[0042] Comparative Example 2

[0043] 0.6 g of iron titanate prepared in Example 3 was placed in a beaker containing 100 ml of a 10 mg / L tetracycline solution, subjected to ultrasonic treatment for 2 minutes, dark adsorbed for 30 minutes, and then illuminated for 60 minutes with a 300-W xenon lamp at a distance of 20 cm from the liquid surface under stirring. The degraded solution was centrifuged and its absorbance at 357 nm was measured by a UV-visible spectrophotometer. The degradation rate of tetracycline was calculated to be 30.7%.

[0044] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing an iron titanate / cerium oxide composite material, It is characterized in that The steps include: (1) Preparation of nano iron titanate: Add an iron source to anhydrous ethanol, stir until completely dissolved, then drop a titanium source, add ethylenediamine dropwise under continuous stirring to form a sol, then perform a hydrothermal reaction, cool, wash with water, wash with alcohol, dry in vacuum, and calcine under inert gas protection to obtain nano iron titanate; (2) Preparation of iron titanate / cerium oxide composite material: adding the nano iron titanate obtained in step (1) to anhydrous ethanol, and then adding octadecylamine, polyvinyl pyrrolidone and a cerium source, stirring and then performing a hydrothermal reaction. The obtained precipitate is washed and then vacuum dried to obtain an iron titanate / cerium oxide composite material; Wherein, in step (1), the hydrothermal reaction conditions are: temperature of 160-200°C, reaction time of 8-24 hours, and calcination conditions are: temperature of 650-700°C, time of 2-3 hours; In step (2), the hydrothermal reaction conditions are: temperature of 160-200° C., and reaction time of 80-120 minutes.

2. The method for preparing the iron titanate / cerium oxide composite material according to claim 1, It is characterized in that In step (1), the iron in the iron source is a positive trivalent ion, and the molar ratio of the iron element in the iron source to the titanium element in the titanium source is 1:

1.

3. The method for preparing the iron titanate / cerium oxide composite material according to claim 1, It is characterized in that In step (1), the iron source is one or more of ferric nitrate, ferric chloride and ferric sulfate.

4. The method for preparing the iron titanate / cerium oxide composite material according to claim 1, It is characterized in that In step (1), the titanium source is tetrabutyl titanate and / or tetraisopropyl titanate.

5. The method for preparing the iron titanate / cerium oxide composite material according to claim 1, It is characterized in that In step (2), the molar ratio of the iron element in the iron titanate to the cerium element in the cerium source is 1-2:2; the mass ratio of octadecylamine to the cerium source is 1-2:10; and the mass ratio of polyvinyl pyrrolidone to the cerium source is 1-2:

2.

6. The iron titanate / cerium oxide composite material prepared by the preparation method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Preparation method and application of iron titanate nano material

    CN112271085A

  • Ferrum-cerium-titanium composite oxide catalyst, preparation method and application of ferrum-cerium-titanium composite oxide catalyst

    CN103071506A

  • Preparation method of FeTiO3 photo-catalyst with hollow spiny ball structure

    CN104324721A

  • Novel graphene-covered titanate compound and preparation method thereof

    CN106634056A

  • Nanometer iron titanate-based magnetic adsorption material, and preparation method and application thereof