Hollow fiber and preparation method thereof, and nanocomposite material
By preparing hollow fibers and combining them with resin, the problem of difficult dispersion of nanomaterials in resin was solved, achieving high orientation and uniform dispersion, and improving the mechanical and electrical properties of the composite material.
Patent Information
- Application Number
- CN202211606458.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-14
AI Technical Summary
Existing technologies make it difficult to uniformly disperse nanomaterials in resins, resulting in low content of nanocomposite reinforcements, poor dispersibility, and poor orientation, which in turn affects the mechanical and electrical properties of the composite materials.
A hollow fiber preparation method is adopted, in which a specific proportion of orientation aids are added and mixed with nanomaterials, and hollow fibers are prepared by coaxial spinning technology. The fibers are then combined with resin by impregnation or vacuum infusion method to achieve high orientation degree and uniform dispersion of nanomaterials.
This improved the mechanical properties and electrical conductivity of nanocomposites, solved the problems of difficult dispersion, low content, and poor orientation of nanomaterials in resins, and enabled the preparation of high-performance composite materials.
Smart Images

Figure CN116254622B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a hollow fiber and a preparation method thereof, and a nano composite material. Background Art
[0002] Nanomaterials, such as carbon nanotubes, graphene, and boron nitride, have excellent mechanical strength, electrical conductivity, and thermal conductivity, as well as low density and high aspect ratio, which make their mechanical, electrical, and thermal properties far superior to carbon fibers. Therefore, they are recognized as the ideal reinforcement phase for lightweight, high-performance composite materials after carbon fibers. A large number of studies have shown that adding CNTs, graphene, etc. to polymer resins can significantly improve the mechanical and electrical properties of polymer resins. However, due to the large specific surface area of nanomaterials, it is difficult to evenly disperse them in the resin matrix, resulting in the performance of nanocomposites being difficult to achieve the expected height. Therefore, how to obtain high-performance nanocomposites has attracted more and more attention.
[0003] In the prior art, nanocomposites are usually prepared by mixing nanoreinforcements with resins through a direct dispersion method, and then pressing them into composite materials using a mold. However, since nanomaterials have a large specific surface area, uniform dispersion in resins is a huge challenge currently faced. Existing methods include the use of dispersants, surface chemical grafting treatment, etc., but dispersants have poor binding properties with resins, and chemical grafting will destroy the structure of the nanomaterials themselves and reduce their performance. Therefore, there is currently no method for uniformly dispersing nanomaterials in resins, and the prepared nanocomposite reinforcements have low content, poor dispersibility, and almost no orientation, so the mechanical and electrical properties are relatively low.
[0004] The preparation method of pre-assembling nanomaterials into macroscopic bodies and then compounding with resin can avoid the problem of difficulty in dispersing nanomaterials in the resin matrix, and can achieve a high content of nano-reinforced bodies in the composite material, thereby improving the performance of the composite material. For example, carbon nanotubes are first prepared into films and then compounded with resin to obtain a carbon nanotube film composite material with a high carbon tube content, but the carbon nanotube film is usually non-oriented, so its composite material also has poor orientation, resulting in poor mechanical properties. The orientation of carbon nanotube films can be improved by methods such as stretching orientation, but the density of oriented films is high, which increases the difficulty of resin impregnation. Highly oriented carbon nanotube films can also be obtained by carbon nanotube array film drawing method, but the preparation process of carbon nanotube arrays is complicated and difficult to mass produce, which greatly limits the application of carbon nanotubes.
[0005] Therefore, developing a nanocomposite reinforcement and a preparation method thereof, improving the orientation of nanomaterials, enabling the nanomaterials to be evenly dispersed in resins, and improving the mechanical properties and conductivity of composite materials are technical problems that need to be solved urgently in this field. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a hollow fiber and a preparation method thereof, and a nano-composite material. The raw material of the hollow fiber is added with an orientation aid, and the orientation aid is compounded with the nano-material in a specific ratio, so that the orientation degree of the nano-material in the fiber can be improved, and the obtained hollow fiber is then combined with the resin by impregnation or vacuum infusion, which effectively avoids the problems of difficult dispersion, low content and poor orientation of the nano-material in the resin; so that the composite material including the hollow fiber has excellent mechanical properties.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a hollow fiber, wherein the raw materials of the hollow fiber include nanomaterials and an orientation aid; the mass ratio of the nanomaterials to the orientation aid is (5-20):1.
[0009] In the present invention, the orientation of the nanomaterial is induced by the orientation of the orientation aid in the system, thereby improving the orientation degree of the nanomaterial; by adjusting the content of the orientation aid, the controllability of the fiber structure and shape can be effectively improved, and the mechanical properties of the hollow fiber can be improved. Preferably, the mass ratio of the nanomaterial to the orientation aid is (5-20):1, for example, it can be 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, etc.
[0010] In the present invention, the mass ratio of the nano material to the orientation aid is within a specific range, the orientation degree of the nano material is higher, and the mechanical properties of the fiber are better.
[0011] Preferably, the nanomaterial includes at least one of carbon nanotubes, graphene, graphene oxide, cellulose or boron nitride.
[0012] Preferably, the length of the carbon nanotubes is 10 to 200 μm, for example, it can be 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, etc., and more preferably 20 to 50 μm.
[0013] Preferably, the carbon nanotubes include single-walled carbon nanotubes and / or multi-walled carbon nanotubes.
[0014] Preferably, the flake diameters of the graphene and graphene oxide are independently 0.5 to 20 μm, for example, 1 μm, 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, etc., more preferably 5 to 15 μm.
[0015] Preferably, the diameter of the cellulose is 10 to 100 nm, for example, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, etc.
[0016] Preferably, the boron nitride includes boron nitride nanosheets and / or boron nitride nanotubes.
[0017] Preferably, the alignment aid comprises at least one of graphene oxide and nanocellulose.
[0018] Preferably, the flake diameter of graphene oxide in the alignment aid is 0.1 to 1 μm, for example, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.7 μm, 0.8 μm, 1 μm, etc., and more preferably 0.2 to 0.5 μm.
[0019] Preferably, the diameter of the nanocellulose in the alignment aid is 2 to 10 nm, for example, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, etc.
[0020] Preferably, the length of the hollow fiber is ≥10 cm, for example, it can be 15 cm, 20 cm, 25 cm, 30 cm, 35 cm, 40 cm, 45 cm, 50 cm, 55 cm, 60 cm, 65 cm, 70 cm, 75 cm, 80 cm, 85 cm, 90 cm, 95 cm, 100 cm, etc.
[0021] Preferably, the wall thickness of the hollow fiber is 2 to 100 μm, for example, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, etc.
[0022] Preferably, the inner diameter of the hollow fiber is 10 to 200 μm, for example, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 80 μm, 100 μm, 120 μm, 140 μm, 160 μm, 180 μm, etc.
[0023] In a second aspect, the present invention provides a method for preparing the hollow fiber according to the first aspect, the preparation method comprising the following steps:
[0024] The nanomaterial is mixed with an orientation aid to obtain a spinning solution; the spinning solution is spun or 3D printed to obtain the hollow fiber.
[0025] Preferably, the nanomaterial is in the form of a nanomaterial dispersion.
[0026] In the present invention, the alignment aid can also adjust the viscosity of the nanomaterial dispersion, which is more conducive to spinning.
[0027] In the present invention, the preparation method of the nano material dispersion comprises: mixing and dispersing the nano material with a dispersant and a solvent to obtain the nano material dispersion.
[0028] Preferably, the dispersant comprises at least one of sodium cholate, sodium dodecyl sulfate or polyvinyl pyrrolidone.
[0029] Preferably, the mixing and dispersing method includes at least one of ultrasonic dispersion, cell crushing or high-pressure homogenization.
[0030] Preferably, the mass percentage of the nanomaterial in the nanomaterial dispersion is 0.1-5%, for example, it can be 0.2%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.4%, 3.8%, 4%, 4.2%, 4.6%, 4.8% and the like.
[0031] Preferably, the spinning comprises coaxial spinning.
[0032] Preferably, the specific steps of the coaxial spinning include: mixing the nanomaterial with an orientation aid to obtain a spinning solution; extruding the spinning solution and an internal coagulation bath, and externally coagulating to obtain the hollow fiber.
[0033] Preferably, the extrusion device comprises a coaxial syringe pump.
[0034] Preferably, the flow rate of the outer hole of the coaxial syringe pump is 35-45 mL / h, for example, it can be 36 mL / h, 37 mL / h, 38 mL / h, 39 mL / h, 40 mL / h, 41 mL / h, 42 mL / h, 43 mL / h, 44 mL / h, etc.
[0035] Preferably, the inner hole flow rate of the coaxial syringe pump is 30-40 mL / h, for example, it can be 31 mL / h, 32 mL / h, 33 mL / h, 34 mL / h, 35 mL / h, 36 mL / h, 37 mL / h, 38 mL / h, 39 mL / h, etc.
[0036] In the present invention, the outer hole flow rate of the coaxial injection pump refers to the flow rate of the spinning solution, and the inner hole flow rate refers to the flow rate of the inner coagulation bath; when the outer hole flow rate and the inner hole flow rate are within a specific range, the prepared hollow fiber is more suitable as a resin reinforcement, thereby improving the mechanical properties of the composite material.
[0037] Preferably, the inner coagulation bath and the outer coagulation bath each independently include at least one of water, methanol, ethanol, isopropanol or acetone.
[0038] Preferably, the inner coagulation bath and the outer coagulation bath each independently include a mixed solvent of water and an organic solvent.
[0039] Preferably, the volume ratio of water to the organic solvent is (0.1-1):1, for example, it can be 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, etc.
[0040] Preferably, the speed of the external coagulation bath is 1200-1800 m / h, for example, 1250 m / h, 1300 m / h, 1350 m / h, 1400 m / h, 1450 m / h, 1500 m / h, 1550 m / h, 1600 m / h, 1650 m / h, 1700 m / h, 1750 m / h, etc.
[0041] In the present invention, the coagulation bath speed refers to the coagulation bath rotation speed.
[0042] Preferably, the step of rolling up and / or drying is further included after solidification.
[0043] Preferably, the winding speed is 1600-2000 m / h, for example, it can be 1650 m / h, 1700 m / h, 1750 m / h, 1800 m / h, 1850 m / h, 1900 m / h, 1950 m / h, 1980 m / h, etc.
[0044] Preferably, the drying temperature is 20-80°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, etc.
[0045] In the present invention, the drying temperature can achieve the regulation of fiber wall thickness and fiber diameter.
[0046] In a third aspect, the present invention provides a nanocomposite material, wherein the nanocomposite material comprises a matrix resin and a nanoreinforcement body; the nanoreinforcement body comprises the hollow fiber as described in the first aspect.
[0047] Preferably, the matrix resin includes a thermosetting resin and / or a thermoplastic resin.
[0048] Preferably, the mass percentage of the hollow fibers in the nanocomposite material is 5-50%, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, etc.
[0049] In the present invention, the preparation method of the nanocomposite material comprises combining the hollow fiber with the resin by impregnation or vacuum infusion to obtain the nanocomposite material.
[0050] In the present invention, the hollow fiber obtained by using a specific raw material ratio and process is used as a resin reinforcement. On the one hand, the outer surface and the inner surface of the hollow fiber can be infiltrated with resin, which reduces the diffusion distance of the resin, thereby achieving uniform mixing of the resin and the nanomaterial. Compared with the traditional solid fiber, the problem of uneven structure caused by the skin-core structure of the solid fiber and the inability of the resin to enter the fiber core is solved. On the other hand, the orientation degree of the nanomaterial in the hollow fiber obtained by the present invention is high, which improves the problem of poor orientation of the nanomaterial in direct dispersion, thin film and traditional solid fiber; at the same time, the high orientation degree can obtain high mechanical and electrical properties, so that the nanomaterial content in the final nanocomposite material is high and can be evenly dispersed, which improves the mechanical properties of the composite material.
[0051] In the present invention, when the nanomaterial is a conductive material, adding an orientation aid in a specific ratio is also beneficial to improving the conductivity of the nanocomposite material.
[0052] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] The hollow fiber provided by the present invention is beneficial to improving the orientation degree of nanomaterials in the fiber by adding a specific content of orientation aid, so as to obtain a hollow fiber with a hollow, porous and highly oriented structure, thereby improving the mechanical properties and electrical properties of the hollow fiber; and the shape and structure of the carbon nanotube hollow fiber are controllable and can be produced continuously, thereby expanding the application of the hollow fiber, increasing the content of nanomaterials in the resin composite material and achieving uniform dispersion of the nanomaterials in the resin, thereby improving the mechanical properties of the resin composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is a scanning electron microscope image of the hollow fiber provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0057] In the present invention, unless otherwise specified, the raw materials of all embodiments and comparative examples are as follows:
[0058] Original carbon nanotubes: OCSiAl single-walled carbon nanotubes;
[0059] Nanocellulose: Nanocellulose with different diameters can be prepared by referring to the method disclosed in the literature (Zhu, H.; Zhu, S.; Jia, Z.; Parvinian, S.; Li, Y.; Vaaland, O.; Hu, L.; Li, T., Anomalous scaling law of strength and toughness of cellulose nanopaper. Proc Natl Acad Sci USA 2015, 112 (29), 8971-8976.);
[0060] Pristine graphene oxide: Jicang JCGO-1-50;
[0061] In the specific embodiment, carbon nanotubes of different lengths and graphene oxide of different sheet diameters can be obtained by oxidizing the original carbon nanotubes and the original graphene oxide or subjecting them to mechanical treatment such as ultrasound.
[0062] Example 1
[0063] This embodiment provides a hollow fiber, the raw materials of which include carbon nanotubes (length: 30 μm) and nanocellulose (diameter: 5 nm); the mass ratio of the carbon nanotubes to the nanocellulose is 20:1.
[0064] This embodiment provides a method for preparing a hollow fiber, which specifically includes the following steps:
[0065] (1) uniformly mixing carbon nanotubes and sodium dodecyl sulfate in water, and ultrasonically dispersing the mixture to prepare a carbon nanotube dispersion (the mass percentage of carbon nanotubes in the carbon nanotube dispersion is 0.4%); adding nanocellulose to the carbon nanotube dispersion to obtain a carbon nanotube spinning stock solution;
[0066] (2) The carbon nanotube spinning stock solution obtained in step (1) and the internal coagulation bath (a mixed solution of water and ethanol in a volume ratio of 0.5:1) are loaded into a coaxial injection pump, and extruded into an external coagulation bath through the coaxial injection pump to form fibers, and then the fibers are rolled up and dried at 60°C to obtain the carbon nanotube hollow fibers; the outer hole flow rate of the coaxial injection pump is 40 mL / h, and the inner hole flow rate is 35 mL / h; the external coagulation bath is a mixed solution of ethanol and water, and the mixed volume ratio is ethanol: water = 1:0.2; the coagulation bath is a rotating coagulation bath, the speed of the coagulation bath is 1300 m / h, and the winding speed is 1700 m / h.
[0067] The morphology of the hollow fiber obtained in Example 1 was characterized by a scanning electron microscope (model: S-4800). Figure 1 shown.
[0068] Example 2
[0069] The present embodiment provides a hollow fiber, the raw materials of which include carbon nanotubes (length of 20 μm) and graphene oxide (sheet diameter of 0.5 μm); the mass ratio of the carbon nanotubes to the graphene oxide is 12:1.
[0070] This embodiment provides a method for preparing a hollow fiber, which specifically includes the following steps:
[0071] (1) uniformly mixing carbon nanotubes and sodium dodecyl sulfate in water, and dispersing by ultrasonication to prepare a carbon nanotube dispersion (the mass percentage of carbon nanotubes in the carbon nanotube dispersion is 1%); adding graphene oxide to the carbon nanotube dispersion to obtain a carbon nanotube spinning stock solution;
[0072] (2) The carbon nanotube spinning stock solution obtained in step (1) and the internal coagulation bath (a mixed solution of water and acetone in a volume ratio of 0.8:1) are loaded into a coaxial syringe pump, and extruded into an external coagulation bath through the coaxial syringe pump to form fibers, and then the fibers are rolled up and dried at 60°C to obtain the carbon nanotube hollow fibers; the outer hole flow rate of the coaxial syringe pump is 35 mL / h, and the inner hole flow rate is 30 mL / h; the external coagulation bath is a mixed solution of isopropanol and water, and the mixing volume ratio is isopropanol: water = 1:0.1, the coagulation bath is a rotating coagulation bath, the speed of the coagulation bath is 1500 m / h, and the winding speed is 1800 m / h.
[0073] Example 3
[0074] The present embodiment provides a hollow fiber, wherein the raw materials of the carbon nanotube hollow fiber include carbon nanotubes (with a length of 50 μm) and graphene oxide (with a sheet diameter of 0.2 μm); the mass ratio of the carbon nanotubes to the graphene oxide is 15:1.
[0075] This embodiment provides a method for preparing a hollow fiber, and the specific steps are the same as those in Embodiment 1.
[0076] Example 4
[0077] The present embodiment provides a hollow fiber, wherein the raw materials of the carbon nanotube hollow fiber include carbon nanotubes (with a length of 40 μm) and graphene oxide (with a sheet diameter of 1 μm); the mass ratio of the carbon nanotubes to the graphene oxide is 18:1.
[0078] This embodiment provides a method for preparing a hollow fiber, and the specific steps are the same as those in Embodiment 1.
[0079] Example 5
[0080] This embodiment provides a hollow fiber, the raw materials of which include graphene oxide (original graphene oxide) and nanocellulose (with a diameter of 10 nm); the mass ratio of the graphene oxide to the nanocellulose is 5:1.
[0081] This embodiment provides a method for preparing a hollow fiber, and the specific steps are the same as those in Embodiment 1.
[0082] Example 6
[0083] This embodiment provides a hollow fiber, which is different from the embodiment 2 only in that the sheet diameter of the graphene oxide is 2 μm, and the amounts of other raw materials, preparation methods and parameters are the same as those in the embodiment 2.
[0084] Example 7
[0085] This embodiment provides a hollow fiber, which is different from the embodiment 2 only in that the sheet diameter of the graphene oxide is 50 nm, and the other raw material amounts, preparation methods and parameters are the same as those in the embodiment 2.
[0086] Example 8
[0087] This embodiment provides a hollow fiber, which is different from the embodiment 1 only in that the diameter of the nanocellulose is 20 nm, and the amounts of other raw materials, preparation methods and parameters are the same as those in the embodiment 1.
[0088] Example 9
[0089] This embodiment provides a hollow fiber, which is different from the embodiment 1 only in that the diameter of the nanocellulose is 1 nm, and the amounts of other raw materials, preparation methods and parameters are the same as those in the embodiment 1.
[0090] Example 10
[0091] This embodiment provides a hollow fiber, which differs from Embodiment 2 only in that, in the preparation method, the outer hole flow rate of the coaxial injection pump in step (2) is 30 mL / h, and the inner hole flow rate is 45 mL / h, and the other raw material amounts, preparation methods and parameters are the same as those in Embodiment 2.
[0092] Embodiment 11
[0093] This embodiment provides a hollow fiber, which differs from Embodiment 2 only in that, in the preparation method, the outer hole flow rate of the coaxial injection pump in step (2) is 50 mL / h, and the inner hole flow rate is 25 mL / h, and the other raw material amounts, preparation methods and parameters are the same as those in Embodiment 2.
[0094] Comparative Example 1
[0095] This comparative example provides a hollow fiber, which is different from Example 2 only in that the mass ratio of the carbon nanotubes to the graphene oxide is 3:1, and the amounts of other raw materials, the preparation method and the parameters are the same as those in Example 2.
[0096] Comparative Example 2
[0097] This comparative example provides a hollow fiber, which is different from Example 2 only in that the mass ratio of the carbon nanotubes to graphene oxide is 25:1, and the amounts of other raw materials, preparation methods and parameters are the same as those in Example 2.
[0098] Comparative Example 3
[0099] This comparative example provides a hollow fiber, which is different from Example 2 only in that the raw materials of the carbon nanotube hollow fiber do not contain graphene oxide, and the amounts of other raw materials, preparation methods and parameters are the same as those in Example 2.
[0100] Comparative Example 4
[0101] This comparative example provides a solid fiber, which differs from Example 2 only in that, in the preparation method, step (2) uses a uniaxial syringe pump with an extrusion flow rate of 5 mL / h, and the other raw material amounts, steps and parameters are the same as those in Example 2.
[0102] Application Example 1
[0103] A nanocomposite material, which comprises, by weight percentage, 92% epoxy resin (Huntsman CY5948 / HY925-1) and 8% hollow fibers (Example 1); a preparation method of the nanocomposite material comprises: dissolving the epoxy resin in acetone with a weight fraction of 6%, dipping the dried hollow fibers into the acetone solution of the epoxy resin, and hot-pressing and curing the hollow fibers at 100° C. to obtain the nanocomposite material.
[0104] Application Example 2
[0105] A nanocomposite material, which comprises, by weight percentage, 90% epoxy resin (Huntsman CY5948 / HY925-1) and 10% hollow fiber (Example 2); a preparation method of the nanocomposite material comprises: dissolving the epoxy resin in acetone with a weight fraction of 6%, dipping the dried hollow fiber into the acetone solution of the epoxy resin, and hot-pressing and curing the hollow fiber at 100°C to obtain the nanocomposite material.
[0106] Application Examples 3 to 11
[0107] Application Examples 3 to 11 provide a nanocomposite material, which differs from Application Example 1 only in that the hollow fibers are the hollow fibers provided in Examples 3 to 11, respectively, and other raw materials, dosages and preparation methods are the same as those in Application Example 1.
[0108] Comparative Application Examples 1 to 3
[0109] Comparative Application Examples 1 to 3 provide a nanocomposite material, which differs from Application Example 1 only in that the hollow fibers are the hollow fibers provided by Comparative Examples 1 to 3, respectively, and other raw materials, dosages and preparation methods are the same as those in Application Example 1.
[0110] Comparative Application Example 4
[0111] Comparative Application Example 4 provides a nanocomposite material, which differs from Application Example 1 only in that the fiber is the solid fiber provided in Comparative Example 4, and other raw materials, dosages and preparation methods are the same as those in Application Example 1.
[0112] Performance Testing
[0113] (1) Tensile strength: Five samples of the same length (1 cm) were tested using an instron 3365 mechanical tensile tester (USA) and the load data were recorded. The cross section of the original fiber was observed using a SEM (S-4800, Hitachi, Japan) and the mechanical tensile strength data was calculated using the strength formula; tensile strength = axial tension / cross-sectional area of the material specimen;
[0114] (2) Conductivity: For each sample (five samples were prepared and the average value was taken), a sample of the same length (1 m) was prepared and the resistance of the sample was tested using an instrument (KEITHLEY INSTRUMENTS 28775AURORA RD.CLEVELAND, OHIO 44139). The conductivity data of the fiber was calculated using the conductivity calculation formula using the cross-sectional data of the SEM mentioned above; conductivity = length of sample to be tested / (resistance * cross-sectional area).
[0115] The specific test results are shown in Table 1:
[0116] Table 1
[0117] Tensile strength(MPa) <![CDATA[Conductivity (S / m) / 10 4 > Application Example 1 368 1.2 Application Example 2 600 12 Application Example 3 450 10.2 Application Example 4 410 8.5 Application Example 5 330 Non-conductive Application Example 6 320 6.5 Application Example 7 315 5.4 Application Example 8 290 0.3 Application Example 9 280 0.7 Application Example 10 260 3.5 Application Example 11 252 2.2 Comparative application example 1 330 7.5 Comparative Application Example 2 288 6.4 Comparative Application Example 3 240 4.8 Comparative Application Example 4 130 5.4
[0118] As can be seen from the above table, the hollow fiber provided by the present invention, by adding a specific content of an orientation aid, is conducive to improving the orientation degree of the nanomaterial in the fiber, and obtaining a hollow fiber with a hollow, porous, and highly oriented structure, so that the resin composite material including the hollow fiber has excellent mechanical and electrical properties. As can be seen from Application Examples 1 to 5, the tensile strength of the nanocomposite material including the hollow fiber is 330 to 600 MPa, and the electrical conductivity is (0 to 12)×10 4 .
[0119] Comparing Application Example 2 with Application Examples 6 and 7, it can be seen that the sheet diameter of the orientation agent graphene oxide is not within the specific range, and the orientation of the carbon nanotubes in the fiber is poor; comparing Application Example 1 with Application Examples 8 and 9, it can be seen that the sheet diameter of the nanocellulose is not within the specific range, the orientation of the carbon nanotubes in the fiber is poor, and the mechanical properties are deteriorated; comparing Application Examples 2 with 10 to 11, it can be seen that the flow rate of the inner and outer holes of the coaxial injection pump in the preparation method is not within the specific range, and the shape of the hollow fiber is difficult to maintain, or it collapses, or there is no hollow structure.
[0120] It can be seen from the comparison between Application Example 2 and Comparative Application Examples 1 to 3 that the hollow fiber does not contain an orientation aid or the orientation aid and the nanomaterial are not in a specific ratio, and the mechanical and electrical properties of the fiber deteriorate.
[0121] It can be seen from Application Example 2 and Comparative Application Example 4 that the hollow fiber provided by the present invention, as a reinforcement for resin, is better than solid fiber in improving the performance of resin.
[0122] In summary, the hollow fiber provided by the present invention, by adding an orientation aid and adopting a specific preparation method, the nanomaterial in the fiber is highly oriented to obtain a hollow, porous fiber with controllable structure. Furthermore, the hollow fiber is compounded with a resin by methods such as impregnation or vacuum infusion, so that the nanomaterial content in the resin composite material is high and evenly dispersed, thereby improving the mechanical properties and mechanical properties of the composite material; and the preparation process of the hollow fiber is simple and can be produced continuously.
[0123] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A hollow fiber, characterized in that: The raw materials of the hollow fiber are composed of nano materials and orientation aids; The mass ratio of the nano material to the alignment aid is (5-20):1; The alignment aid comprises at least one of graphene oxide and nanocellulose; The sheet diameter of graphene oxide in the alignment aid is 0.1 to 1 μm; The diameter of the nanocellulose in the alignment aid is 2 to 10 nm; The nanomaterial is a carbon nanotube; The hollow fiber is prepared by the following method, which comprises the following steps: After mixing the nano material with the orientation aid, a spinning solution is obtained; and the spinning solution is spun to obtain the hollow fiber; The nanomaterial is present in the form of a nanomaterial dispersion; The spinning is coaxial spinning.
2. The hollow fiber according to claim 1, characterized in that The length of the carbon nanotube is 10 to 200 μm.
3. The hollow fiber according to claim 2, characterized in that The length of the carbon nanotube is 20-50 μm.
4. The hollow fiber according to claim 1, characterized in that The length of the hollow fiber is ≥10 cm.
5. The hollow fiber according to claim 1, characterized in that The wall thickness of the hollow fiber is 2-100 μm.
6. A method for preparing a hollow fiber according to any one of claims 1 to 5, characterized in that: The preparation method The steps include: After mixing the nano material with the orientation aid, a spinning solution is obtained; and the spinning solution is spun to obtain the hollow fiber; The nanomaterial is present in the form of a nanomaterial dispersion; The spinning is coaxial spinning.
7. The preparation method according to claim 6, characterized in that: The mass percentage of the nano material in the nano material dispersion is 0.1-5%.
8. A nanocomposite material, characterized in that: The nanocomposite material comprises a matrix resin and a nanoreinforcement; the nanoreinforcement comprises the hollow fiber as claimed in any one of claims 1 to 5.
9. The composite material according to claim 8, characterized in that The matrix resin includes a thermosetting resin and / or a thermoplastic resin.
10. The composite material according to claim 8, characterized in that The mass percentage of the nano-reinforcement in the composite material is 5-50%.