A method for preparing furandicarboxylic acid polyester

By using a combination of zinc and titanium or stannous catalysts in the preparation of furandiformic acid polyester, the polycondensation temperature and conditions are controlled, and the problems of long solid phase polycondensation time and color in the prior art are solved, and high molecular weight and light color are achieved. The rapid preparation of furandicarboxylic acid polyester reduces production costs and improves product quality.

CN116262819BActive Publication Date: 2024-11-12ZHEJIANG HENGYI PETROCHEMICAL RES INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211557256.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-11-12
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to prepare furandicarboxylic acid polyester with high molecular weight and light color in a short time, resulting in too long solid phase polycondensation time and making it difficult to achieve industrial production.

Method used

Use zinc as a separate polycondensation catalyst for melt polycondensation at a lower temperature, and then add highly active titanium or stannous catalysts, and gradually increase the temperature during the solid phase polycondensation process, control the reaction conditions to avoid discoloration and shorten the solid phase polycondensation time .

Benefits of technology

It has achieved the preparation of high molecular weight furandicarboxylic acid polyester in a short time, with a characteristic viscosity reaching 0.75-1.20dL/g and an absorbance less than 0.02, reducing production costs and improving product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003983183280000121
    Figure BDA0003983183280000121
Patent Text Reader

Abstract

The present invention relates to the field of polyester preparation, and aims at the problem that furandicarboxylic acid polyester with high molecular weight and light color is difficult to synthesize by solid phase polycondensation, and provides a method for preparing furandicarboxylic acid polyester, comprising the steps of: furandicarboxylic acid or furandicarboxylic acid diester and diol are subjected to esterification or transesterification reaction under the action of a first catalyst to obtain a product P1; P1 is subjected to melt polycondensation reaction at 220-250°C and <50Pa for 2-6h to obtain a polyester prepolymer P2; normal pressure is restored, a second catalyst or a polyester masterbatch P3 containing the second catalyst is added to P2 and mixed uniformly; granulation and pre-crystallization treatment are performed to obtain polyester prepolymer pellets P4 containing the second catalyst; P4 is subjected to solid phase polycondensation at a temperature lower than its melting point in a vacuum or inert gas flow to obtain a product. The present invention combines the discoloration inhibition of the first catalyst and the high activity of the second catalyst to obtain a furandicarboxylic acid polyester with high molecular weight and light color in a relatively short time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polyester preparation, in particular to a method for preparing furandicarboxylic acid polyester. Background Art

[0002] Furandicarboxylic acid polyesters, produced by polymerizing the bio-based monomers 2,5-furandicarboxylic acid (FDCA) or dimethyl 2,5-furandicarboxylate (DMFD) with diols, are a class of bio-based polymers. Compared to traditional terephthalate-based polyesters, furandicarboxylic acid polyesters not only possess superior thermo-mechanical properties and gas barrier properties but also, in today's increasingly prominent environmental and resource issues, are of great significance in mitigating the greenhouse effect and conserving petrochemical resources. Among these, poly(ethylene 2,5-furandicarboxylate) (PEF) has garnered the most attention. However, due to the difficulty of monomer purification, poor thermal stability, the susceptibility to side reactions during the reaction, and the lack of highly active and selective catalysts, the preparation of furandicarboxylic acid polyesters via melt polycondensation often struggles to achieve both molecular weight improvement and discoloration control. Consequently, the resulting products fail to meet the demands for manufacturing high-quality polyester bottles, fibers, and films.

[0003] Solid-phase polycondensation (SSP) is a common technique for further increasing the molecular weight of semi-crystalline polymers by further polycondensing them in a solid state at relatively low temperatures (below their melting point). Due to the low polymerization temperature, SSP can effectively avoid side reactions such as discoloration. SSP is also widely used in the synthesis of polyether ... For example, in patent WO2010077133, it takes 60 hours of solid phase polycondensation to increase the molecular weight of PEF to 34,000 g / mol, and in patent CN106916287A, it takes 24 hours to increase the intrinsic viscosity of PEF from 0.253 dL / g to 0.724 dL / g. For another example, Journal of Polymer Science Part A: Polymer Chemistry (51(19):4191-4199, 2013) reported that it takes 72 hours of solid phase polycondensation to reach a molecular weight of 83,000 g / mol of PEF; and Green Chemistry (18(19):5142-5150, 2016) reported that after 48 hours of solid phase polycondensation, the intrinsic viscosity of PEF with an intrinsic viscosity of 0.60 dL / g only increased to 0.72 dL / g. It can be seen that the time required for these solid phase polycondensation processes is longer than 24 hours, and such a long reaction time makes it difficult to industrialize production.

[0004] Patent WO2013062408 discloses a method for preparing light-colored PEF. By adding a zinc or calcium catalyst during the transesterification stage and an antimony catalyst during the polycondensation stage, the resulting PEF has a number-average molecular weight of 17,900 g / mol and an absorbance of 0.007 at 400 nm. After 24 hours of solid-state polycondensation, the number-average molecular weight reaches 45,500 g / mol, with an absorbance of <0.05. Patent WO2015137806 states that appropriately increasing the carboxyl group content (CC) of the PEF prepolymer can help increase the solid-state polycondensation rate and significantly shorten the solid-state polycondensation time. The intrinsic viscosity of the PEF increases from 0.488 dL / g to 0.774 dL / g in just 8 hours, with an intrinsic viscosity growth rate of 0.036 dL / g / h. However, the color change during the polymerization process is not mentioned. Patent WO2017048119 proposes a method of adding FDCA during the polycondensation stage to increase CC, further shortening the time to increase the number average molecular weight from 15,000-18,000 g / mol to approximately 30,000 g / mol to 6-7 hours. The patent gives the absorbance of the PEF prepolymer (the absorbance of the PEF prepolymer synthesized using a zinc and antimony composite catalyst is 0.006-0.013, while the absorbance of the PEF prepolymer synthesized using a titanium catalyst is as high as 0.013-0.056), but does not mention the color or absorbance results after solid-phase polycondensation.

[0005] In summary, the current synthesis of furandicarboxylic acid polyesters with both high molecular weight and light color using solid-state polycondensation remains difficult. Either the solid-state polycondensation rate is low, resulting in a long timeframe and hindering industrialization, while also causing discoloration. Alternatively, the prepolymer is light in color, allowing for a faster solid-state polycondensation rate, allowing for a high molecular weight or intrinsic viscosity to be achieved in a shorter timeframe, but significant discoloration still occurs during the solid-state polycondensation process. Synthesizing furandicarboxylic acid polyesters with both high molecular weight and light color using solid-state polycondensation remains a pressing technical challenge. Summary of the Invention

[0006] In order to overcome the problem that it is still difficult to synthesize furandicarboxylic acid polyesters with both high molecular weight and light color by solid phase polycondensation, the present invention provides a method for preparing furandicarboxylic acid polyesters. The method can prepare furandicarboxylic acid polyesters with both high molecular weight and light color within a relatively short solid phase polycondensation time, thereby meeting the requirements of bottle blowing processing.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0009] (1) Esterification or transesterification: furandicarboxylic acid or furandicarboxylic acid diester and diol are subjected to esterification or transesterification reaction at 160-200° C. for 2-6 hours in the presence of a first catalyst to obtain an esterification or transesterification product P1;

[0010] (2) Melt polycondensation: The esterification or transesterification product P1 is subjected to melt polycondensation reaction at 220-250°C and <50 Pa for 2-6 hours to obtain a polyester prepolymer P2;

[0011] (3) Pretreatment: Release the vacuum, return to normal pressure, add the second catalyst or the polyester masterbatch P3 containing the second catalyst to the polyester prepolymer P2, and mix them evenly; then granulate and pre-crystallize the mixture to obtain polyester prepolymer pellets P4 containing the second catalyst;

[0012] (4) Solid phase polycondensation: The polyester prepolymer pellets P4 containing the second catalyst are placed in a vacuum condition or in an inert gas flow at a temperature below the melting point T m Solid phase polycondensation is carried out at a temperature of 500 to obtain the product furandicarboxylic acid polyester.

[0013] Preferably, the furandicarboxylic acid in step (1) is 2,5-furandicarboxylic acid, and the furandicarboxylic acid diester is 2,5-furandicarboxylic acid diester; and the diol is selected from at least one of ethylene glycol, propylene glycol, and butanediol.

[0014] Preferably, in step (1), the first catalyst is a zinc metal compound selected from one or more of zinc oxide, zinc acetate, zinc lactate, zinc acetylacetonate, zinc citrate, and zinc carbonate, preferably one or more of zinc oxide, zinc acetate, and zinc citrate; the amount of the first catalyst used is 0.01-0.2 wt%, preferably 0.05-0.1 wt%, of the total mass of furandicarboxylic acid or furandicarboxylic acid diester and diol.

[0015] Zinc, as a highly efficient transesterification or esterification catalyst, typically requires combination with a secondary metal catalyst, such as titanium, tin, antimony, zirconium, or germanium, to produce high-molecular-weight polyester. However, the inventors have discovered that zinc can also be used alone as a polycondensation catalyst. At higher polycondensation temperatures, the intrinsic viscosity of PEF can be increased to over 0.7 dL / g, albeit with noticeable discoloration. To ensure superior polyester color, the present invention utilizes a lower polycondensation temperature (220-250°C), resulting in an intrinsic viscosity of 0.4-0.7 dL / g, preferably 0.45-0.65 dL / g, for the polyester prepolymer pellets P4.

[0016] Preferably, in step (3), the second catalyst is selected from a titanium compound and / or a stannous compound, the titanium compound is selected from one or more of tetrabutyl titanate, isopropyl titanate, tetraethyl titanate, titanium ethylene glycol, and titanium acetylacetonate, preferably one or more of tetrabutyl titanate, isopropyl titanate, and titanium ethylene glycol; the stannous compound is selected from one or more of stannous acetate, stannous oxalate, stannous octoate, stannous chloride, stannous bromide, and stannous oxide, preferably one or more of stannous oxalate, stannous octoate, and stannous oxide; the amount of the second catalyst is 0.003-0.25 wt%, preferably 0.01-0.15 wt%, of the total mass of furandicarboxylic acid or furandicarboxylic acid diester and diol.

[0017] Compared with the first catalyst, the second catalyst has higher catalytic activity and is more conducive to increasing the molecular weight of the polyester, but it is more likely to cause discoloration at high temperatures. Therefore, the present invention proposes a method of adding the catalyst after the end of melt polycondensation and before solid-phase polycondensation. This method not only avoids the titanium and stannous catalysts from being in contact with the polyester melt for a long time at a higher melt polycondensation temperature, which may cause discoloration of the polyester, but also enables them to exert their high catalytic activity at a lower solid-phase polycondensation temperature, thereby significantly increasing the molecular weight of the polyester.

[0018] Preferably, the polyester masterbatch P3 containing the second catalyst in step (3) is prepared by adding the second catalyst to the polyester prepolymer P2, wherein the amount of the second catalyst is 0.3-3 wt% of the total mass of furandicarboxylic acid or furandicarboxylic acid diester and diol, and stirring for 5-30 minutes to uniformly mix the second catalyst and the polyester prepolymer P2, thereby obtaining the furandicarboxylic acid polyester masterbatch P3 containing the second catalyst. In order to more effectively mix the second catalyst and the polyester prepolymer P2, the present invention also provides a method for mixing the polyester masterbatch P3 containing the second catalyst with the polyester prepolymer P2, wherein the two have similar melt viscosities, which facilitates uniform mixing.

[0019] Preferably, the pre-crystallization treatment conditions in step (3) are 70-200° C. for 0.5-6 h.

[0020] Preferably, the polyester prepolymer pellets P4 containing the second catalyst obtained in step (3) have a particle size of 0.2-3 mm, preferably 0.2-1 mm, and an intrinsic viscosity of not less than 0.4 dL / g, preferably 0.4-0.7 dL / g, and more preferably 0.45-0.65 dL / g.

[0021] Preferably, the solid phase polycondensation in step (4) gradually increases the temperature at a heating rate of 1-5°C / min, so that it is always 5-20°C lower than the melting point of the furandicarboxylic acid polyester, and the solid phase polycondensation time is 3-20h. The preparation method of furandicarboxylic acid polyester is to gradually increase the solid phase polycondensation temperature. The closer the solid phase polycondensation temperature is to the melting point, the more conducive it is to the growth of molecular weight, but it is also easy to cause the polyester pellets to stick or clumping. Therefore, in the solid phase polycondensation process of the present invention, it is necessary to gradually increase the reaction temperature and always keep the reaction temperature close to and 5-20°C lower than its melting point, preferably 5-10°C. This can not only meet the demand for rapid growth of polyester molecular weight, but also prevent pellets from sticking.

[0022] Preferably, the furandicarboxylic acid polyester obtained in step (4) has an intrinsic viscosity of 0.75-1.20 dL / g, and can reach a value of 0.75 dL / g or higher, preferably 0.85 dL / g or higher, within 4-10 hours. A 5 mg / mL solution of the furandicarboxylic acid polyester in a dichloromethane / hexafluoroisopropanol (8:2) volume ratio has an absorbance of less than 0.02 at 400 nm.

[0023] Therefore, the beneficial effects of the present invention are as follows: (1) the present invention rapidly mixes the molten polycondensation product with the highly active second catalyst and then performs solid-phase polycondensation, thereby shortening the solid-phase polycondensation time from tens of hours to less than ten hours (or even 4 hours), greatly shortening the solid-phase polycondensation time, and being beneficial to reducing the cost of industrial solid-phase polycondensation of furandicarboxylic acid polyester; (2) the present invention adopts the first catalyst that is beneficial to suppressing discoloration for melt polycondensation, effectively avoiding discoloration of furandicarboxylic acid polyester during the reaction process, and can prepare high-molecular-weight furandicarboxylic acid polyester with a light color and an absorbance of less than 0.02, thereby improving the quality of furandicarboxylic acid polyester. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below through specific embodiments.

[0025] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art.

[0026] Overall embodiment

[0027] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0028] (1) Esterification or transesterification: furandicarboxylic acid or one of furandicarboxylic acid diesters and a diol are subjected to an esterification or transesterification reaction at 160-200° C. for 2-6 hours in the presence of a first catalyst to obtain an esterification or transesterification product P1;

[0029] The furandicarboxylic acid is 2,5-furandicarboxylic acid, and the furandicarboxylic acid diester is 2,5-furandicarboxylic acid diester. The diol is selected from at least one of ethylene glycol, propylene glycol, and butanediol. The first catalyst is a zinc metal compound selected from one or more of zinc oxide, zinc acetate, zinc lactate, zinc acetylacetonate, zinc citrate, and zinc carbonate, preferably one or more of zinc oxide, zinc acetate, and zinc citrate. The amount of the first catalyst used is 0.01-0.2 wt%, preferably 0.05-0.1 wt%, of the total mass of the furandicarboxylic acid or furandicarboxylic acid diester and the diol.

[0030] (2) Melt polycondensation: The esterification or transesterification product P1 is subjected to melt polycondensation reaction at 220-250°C and <50Pa for 2-6 hours to obtain a polyester prepolymer P2.

[0031] (3) Pretreatment: Release the vacuum, return to normal pressure, add the second catalyst or the polyester masterbatch P3 containing the second catalyst to the polyester prepolymer P2, and stir for 5-30 minutes to uniformly mix the second catalyst or the polyester masterbatch P3 containing the second catalyst with the polyester prepolymer P2; then granulate and pre-crystallize the mixture to obtain polyester prepolymer pellets P4 containing the second catalyst;

[0032] The second catalyst is selected from a titanium compound and / or a stannous compound, the titanium compound is selected from one or more of tetrabutyl titanate, isopropyl titanate, tetraethyl titanate, titanium ethylene glycol, and titanium acetylacetonate, preferably one or more of tetrabutyl titanate, isopropyl titanate, and titanium ethylene glycol; the stannous compound is selected from one or more of stannous acetate, stannous oxalate, stannous octoate, stannous chloride, stannous bromide, and stannous oxide, preferably one or more of stannous oxalate, stannous octoate, and stannous oxide; the amount of the second catalyst is 0.003-0.25 wt%, preferably 0.01-0.15 wt%, based on the total mass of furandicarboxylic acid or furandicarboxylic acid diester and diol;

[0033] The preparation method of the polyester masterbatch P3 containing the second catalyst comprises: adding the second catalyst to the polyester prepolymer P2, wherein the amount of the second catalyst is 0.3-3 wt% of the total mass of furandicarboxylic acid or furandicarboxylic acid diester and diol, and stirring for 5-30 minutes to uniformly mix the second catalyst and the polyester prepolymer P2, thereby obtaining the furandicarboxylic acid polyester masterbatch P3 containing the second catalyst;

[0034] The pre-crystallization treatment condition is 70-200° C. for 0.5-6 hours;

[0035] The obtained polyester prepolymer pellets P4 containing the second catalyst have a particle size of 0.2-3 mm, preferably 0.2-1 mm, and an intrinsic viscosity of not less than 0.4 dL / g, preferably 0.4-0.7 dL / g, and more preferably 0.45-0.65 dL / g.

[0036] (4) Solid phase polycondensation: The polyester prepolymer pellets P4 containing the second catalyst are placed in a vacuum condition or in an inert gas flow at a temperature below the melting point T m solid phase polycondensation at a temperature of 1000 to obtain a product, furandicarboxylic acid polyester;

[0037] The solid phase polycondensation gradually increases the temperature at a heating rate of 1-5°C / min, so that it is always 5-20°C lower than the melting point of furandicarboxylic acid polyester, preferably 5-10°C, and the solid phase polycondensation time is 3-20h.

[0038] The resulting furandicarboxylic acid polyester has an intrinsic viscosity of 0.75-1.20 dL / g, which can reach above 0.75 dL / g, preferably above 0.85 dL / g, within 4-10 hours. A 5 mg / mL solution of the furandicarboxylic acid polyester in a dichloromethane / hexafluoroisopropanol (8:2) volume ratio has an absorbance of less than 0.02 at 400 nm.

[0039] Example 1

[0040] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0041] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0042] (2) Melt polycondensation: Raise the temperature to 230°C and gradually reduce the pressure to below 50 Pa within 30 minutes. Melt polycondensation reaction for 3 hours.

[0043] (3) Pretreatment: Release the vacuum, return the reaction system to normal pressure, add titanium glycolate (0.008 wt% of the total mass of DMFD and ethylene glycol), and continue stirring at 230°C for 15 min to fully disperse the titanium glycolate in the PEF melt. Cool the PEF melt, crush, and sieve to obtain particles with a particle size of 0.2-0.8 mm. Then, place the particles in a vacuum oven at a pressure of <150 Pa, first vacuum dry at 110°C for 1.5 h, and then increase the temperature to 140°C for pre-crystallization for 1 h to obtain PEF prepolymer pellets containing the catalyst titanium glycolate;

[0044] (4) Solid-phase polycondensation: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 3.5 h, high molecular weight PEF was obtained.

[0045] Example 2

[0046] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0047] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0048] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the melt polycondensation reaction was carried out for 3 hours;

[0049] (3) Pretreatment: The reaction system was then returned to normal pressure, titanium glycolate was added (in an amount of 0.016 wt% of the total mass of DMFD and ethylene glycol), and stirring was continued at 230°C for 15 min to fully disperse the titanium glycolate in the PEF melt. The PEF melt was cooled, crushed, and sieved to obtain particles with a particle size of 0.2-0.8 mm. The particles were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 110°C for 1.5 h, and then the temperature was raised to 140°C for pre-crystallization for 1 h to obtain PEF prepolymer pellets containing the catalyst titanium glycolate;

[0050] (4) Solid-phase polycondensation: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 3 h, high molecular weight PEF was obtained.

[0051] Example 3

[0052] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0053] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0054] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the melt polycondensation reaction was carried out for 3 hours;

[0055] (3) Pretreatment: The reaction system was then returned to normal pressure, titanium glycolate was added (in an amount of 0.025 wt% of the total mass of DMFD and ethylene glycol), and stirring was continued at 230°C for 15 min to fully disperse the titanium glycolate in the PEF melt. The PEF melt was cooled, crushed, and sieved to obtain particles with a particle size of 0.2-0.8 mm. The particles were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 110°C for 1.5 h, and then the temperature was raised to 140°C for pre-crystallization for 1 h to obtain PEF prepolymer pellets containing the catalyst titanium glycolate;

[0056] (4) Solid-phase polycondensation: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 4 h, high molecular weight PEF was obtained.

[0057] Example 4

[0058] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0059] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0060] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the melt polycondensation reaction was carried out for 3 hours;

[0061] (3) Pretreatment: The reaction system was then restored to normal pressure, and tetrabutyl titanate (0.05 wt% of the total mass of DMFD and ethylene glycol) was added. Stirring was continued at 230°C for 15 min to fully disperse the tetrabutyl titanate in the PEF melt. The PEF melt was cooled, crushed, and sieved to obtain particles with a particle size of 0.2-0.8 mm. The particles were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 110°C for 1.5 h, and then the temperature was raised to 140°C for pre-crystallization for 1 h to obtain PEF prepolymer pellets containing the catalyst tetrabutyl titanate.

[0062] (4) Solid-phase polycondensation: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 4 h, high molecular weight PEF was obtained.

[0063] Example 5

[0064] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0065] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0066] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the melt polycondensation reaction was carried out for 3 hours;

[0067] (3) Pretreatment: The reaction system was then restored to normal pressure, and stannous octoate (0.15 wt% of the total mass of DMFD and ethylene glycol) was added. Stirring was continued at 230°C for 15 min to fully disperse the stannous octoate in the PEF melt. The PEF melt was cooled, crushed, and sieved to obtain particles with a particle size of 0.2-0.8 mm. The particles were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 110°C for 1.5 h, and then the temperature was raised to 140°C for pre-crystallization for 1 h to obtain PEF prepolymer pellets containing the catalyst stannous octoate.

[0068] (4) Solid-phase polycondensation step: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140°C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210°C at a heating rate of 1°C / min. After solid-phase polycondensation at this temperature for 4 hours, high molecular weight PEF was obtained.

[0069] Example 6

[0070] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0071] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0072] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the melt polycondensation reaction was carried out for 3 hours;

[0073] (3) Pretreatment: The reaction system was then returned to normal pressure, titanium glycolate was added (in an amount of 0.016 wt% of the total mass of DMFD and ethylene glycol), and stirring was continued at 230°C for 15 min to fully disperse the titanium glycolate in the PEF melt. The PEF melt was cooled, crushed, and sieved to obtain particles with a particle size of 0.2-0.8 mm. The particles were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 110°C for 1.5 h, and then the temperature was raised to 140°C for pre-crystallization for 1 h to obtain PEF prepolymer pellets containing the catalyst titanium glycolate;

[0074] (4) Solid-phase polycondensation step: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140°C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 220°C at a heating rate of 1.3°C / min. After solid-phase polycondensation at this temperature for 3 h, high molecular weight PEF was obtained.

[0075] Example 7

[0076] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0077] (1) Transesterification: 73.6 g DMFD, 45.6 g propylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and propylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, and then at 190°C until no more methanol was distilled;

[0078] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the melt polycondensation reaction was carried out for 3 hours;

[0079] (3) Pretreatment: The reaction system was then restored to normal pressure, titanium glycolate (0.016 wt% of the total mass of DMFD and propylene glycol) was added, and stirring was continued at 230°C for 15 min to fully disperse the titanium glycolate in the poly(propylene furandicarboxylate) (PPF) melt. The PPF melt was cooled, crushed, and sieved to obtain particles with a particle size of 0.2-0.8 mm. The particles were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 70°C for 1.5 h, and then the temperature was raised to 130°C for pre-crystallization for 1 h to obtain PPF prepolymer pellets containing the catalyst titanium glycolate;

[0080] (4) Solid-phase polycondensation: The PPF prepolymer pellets were placed in a vacuum oven with a preset temperature of 130°C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 175°C at a heating rate of 0.75°C / min. After solid-phase polycondensation at this temperature for 4 hours, high molecular weight PPF was obtained.

[0081] Example 8

[0082] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0083] (1) Transesterification: 73.6 g DMFD, 54.0 g butanediol, and zinc acetate (0.075 wt% of the total mass of DMFD and butanediol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, and then at 190°C until no more methanol was distilled;

[0084] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the melt polycondensation reaction was carried out for 3 hours;

[0085] (3) Pretreatment: The reaction system was then restored to normal pressure, titanium glycolate (0.016 wt% of the total mass of DMFD and butanediol) was added, and stirring was continued at 230°C for 15 min to fully disperse the titanium glycolate in the polybutylene furandicarboxylate (PBF) melt. The PBF melt was cooled, crushed, and sieved to obtain particles with a particle size of 0.2-0.8 mm. The particles were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 60°C for 1.5 h, and then the temperature was raised to 110°C for pre-crystallization for 1 h to obtain PPF prepolymer pellets containing the catalyst titanium glycolate;

[0086] (4) Solid-phase polycondensation: The PBF prepolymer pellets were placed in a vacuum oven with a preset temperature of 110 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 175 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 4 h, high molecular weight PBF was obtained.

[0087] Example 9

[0088] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0089] (1) Transesterification: 62.4 g of FDCA, 49.6 g of ethylene glycol, and zinc oxide (0.025 wt% of the total mass of FDCA and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0090] (2) Melt polycondensation: the temperature was raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes. The melt polycondensation reaction was carried out for 4 hours to obtain a polyester prepolymer.

[0091] (3) Pretreatment: Release the vacuum, return the reaction system to normal pressure, add a polyester masterbatch containing stannous acetate at 5 wt% of the total mass of FDCA and ethylene glycol, and continue stirring at 230°C for 15 min to achieve uniform dispersion. Cool the melt, crush, and sieve to obtain particles with a particle size of 0.2-0.8 mm. Then, place the particles in a vacuum oven at a pressure of <150 Pa, first vacuum dry at 110°C for 1.5 h, and then increase the temperature to 140°C for pre-crystallization for 1 h to obtain prepolymer pellets.

[0092] The preparation method of the polyester masterbatch containing stannous acetate comprises: adding stannous acetate to the polyester prepolymer of step (2), wherein the amount of stannous acetate is 2 wt% of the total mass of FDCA and ethylene glycol, and stirring for 20 minutes to uniformly mix, thereby obtaining the polyester masterbatch containing stannous acetate;

[0093] (4) Solid-phase polycondensation: The prepolymer pellets were placed in a vacuum oven with a preset temperature of 140 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 4 h, high molecular weight PEF was obtained.

[0094] Comparative Example 1 (Titanium glycolate was added before polycondensation, resulting in a darker color)

[0095] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0096] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0097] (2) Melt polycondensation: Titanium ethylene glycol was then added (the amount was 0.025 wt% of the total mass of DMFD and ethylene glycol), the temperature was raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the polycondensation reaction was continued for 3 hours.

[0098] (3) Pretreatment: The PEF melt was cooled, crushed, and sieved to obtain pellets with a particle size of 0.2-0.8 mm. The pellets were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 110°C for 1.5 h, and then the temperature was raised to 140°C for pre-crystallization for 1 h.

[0099] (4) Solid-phase polycondensation: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 4 h, high molecular weight PEF was obtained.

[0100] Comparative Example 2 (using only a single catalyst, tetrabutyl titanate, resulting in a darker color)

[0101] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0102] (1) Transesterification: 73.6 g of DMFD, 49.6 g of ethylene glycol, and tetrabutyl titanate (the amount used is 0.05 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0103] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the polycondensation reaction was continued for 3 hours.

[0104] (3) Pretreatment: The PEF melt was cooled, crushed, and sieved to obtain pellets with a particle size of 0.2-0.8 mm. The pellets were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 110°C for 1.5 h, and then the temperature was raised to 140°C for pre-crystallization for 1 h.

[0105] (4) Solid-phase polycondensation step: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140°C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210°C at a heating rate of 1°C / min. After solid-phase polycondensation at this temperature for 4 hours, high molecular weight PEF was obtained.

[0106] Comparative Example 3 (using only the first catalyst without adding the second catalyst, the intrinsic viscosity increases slowly)

[0107] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0108] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0109] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the polycondensation reaction was continued for 3 hours.

[0110] (3) Pretreatment: The PEF melt was cooled, crushed, and sieved to obtain pellets with a particle size of 0.2-0.8 mm. The pellets were then placed in a vacuum oven at a pressure of <150 Pa, first vacuum-dried at 110°C for 1.5 h, and then the temperature was raised to 140°C for pre-crystallization for 1 h.

[0111] (4) Solid-phase polycondensation: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 4 h, high molecular weight PEF was obtained.

[0112] Comparative Example 4 (using antimony catalyst instead of the second catalyst, the intrinsic viscosity increases slowly)

[0113] A method for preparing furandicarboxylic acid polyester comprises the following steps:

[0114] (1) Transesterification: 73.6 g DMFD, 49.6 g ethylene glycol, and zinc acetate (0.075 wt% of the total mass of DMFD and ethylene glycol) were added to a reactor protected by nitrogen, and the reaction was carried out at 180°C for 1 h, then at 190°C for 1 h, and then at 200°C until no more methanol was distilled;

[0115] (2) Melt polycondensation: The temperature was then raised to 230°C, and the pressure was gradually reduced to below 50 Pa within 30 minutes, and the melt polycondensation reaction was carried out for 3 hours;

[0116] (3) Pretreatment: The reaction system was then returned to normal pressure, and antimony oxide (0.15 wt% of the total mass of DMFD and ethylene glycol) was added. Stirring was continued at 230°C for 15 min to fully disperse the antimony oxide in the PEF melt. The PEF melt was cooled, crushed, and sieved to obtain particles with a particle size of 0.2-0.8 mm. The particles were then placed in a vacuum oven at a pressure of <150 Pa, vacuum-dried at 110°C for 1.5 h, and then pre-crystallized at 140°C for 1 h to obtain PEF prepolymer pellets containing catalyst antimony oxide.

[0117] (4) Solid-phase polycondensation: The PEF prepolymer pellets were placed in a vacuum oven with a preset temperature of 140 °C, the pressure was reduced to <50 Pa, and the temperature was gradually increased to 210 °C at a heating rate of 1 °C / min. After solid-phase polycondensation at this temperature for 4 h, high molecular weight PEF was obtained.

[0118] Characterization Test

[0119] The test analysis method is as follows:

[0120] Intrinsic viscosity: The test was conducted using a Hangzhou Zhongwang IVS300 semi-automatic viscometer and an Ubbelohde viscometer with a capillary inner diameter of 0.88 mm at a constant temperature of 25°C. The solvent was a phenol / tetrachloroethane mixed solution (mass ratio 3 / 2) with a concentration of 0.5 g / dL.

[0121] Absorbance A400: The absorbance of a 5 mg / mL solution at 400 nm was measured using a TU-1901 double-beam UV-visible spectrophotometer from Puxi General Instrument Co., Ltd. in Beijing, China. The solvent was a mixed solvent of dichloromethane and hexafluoroisopropanol with a volume ratio of 8:2.

[0122]

[0123] a Catalyst abbreviations: ZnAc zinc acetate, ZnO zinc oxide, TEG titanium glycol, TBT n-butyl titanate, Sb2O3 antimony oxide, SnOc stannous octoate, SnAc stannous acetate; "mnp" represents the catalyst added before the transesterification or esterification stage, before the melt polycondensation, and after the melt polycondensation, and the amount thereof. The amount is represented by the number in the brackets and is defined as the mass percentage of the catalyst to the total amount of DMFD and diol, in units of wt%; b : refers to the solid phase polycondensation time, the unit is h; c : intrinsic viscosity of the prepolymer, in dL / g; d : intrinsic viscosity of the solid phase polycondensation product, unit is dL / g; e : the rate of increase of intrinsic viscosity of polyester during solid phase polycondensation, in dL / g / h; f : The commas before and after refer to the absorbance of the prepolymer and the solid-phase polycondensation product at 400 nm, respectively. The solvent is dichloromethane / hexafluoroisopropanol in a volume ratio of 8:2, and the solution concentration is 5 mg / mL.

[0124] The results are shown in the table above. As can be seen from the data in the table, each example utilizes the present method to prepare furandicarboxylic acid polyesters. The method employs a first catalyst that effectively suppresses discoloration for melt polycondensation, and the resulting product is rapidly mixed with a highly active second catalyst before undergoing solid-phase polycondensation. This shortens the solid-phase polycondensation time from tens of hours to less than ten hours (or even four hours), achieving an intrinsic viscosity of 0.75 dL / g or greater within 4-10 hours. Furthermore, discoloration of the furandicarboxylic acid polyester during the reaction is effectively prevented, resulting in a light-colored, high-molecular-weight furandicarboxylic acid polyester with an absorbance of less than 0.02. This method improves the quality of the furandicarboxylic acid polyester and reduces its production cost.

[0125] Compared with Example 1: In Comparative Example 1, titanium glycol was added after the end of the transesterification and before the melt polycondensation, and in Comparative Example 2, only tetrabutyl titanate was used as a single catalyst, and the obtained furandicarboxylic acid polyester had a darker color; in Comparative Example 3, only the first catalyst was used without the second catalyst, and in Comparative Example 4, an antimony catalyst was used instead of the second catalyst, and the intrinsic viscosity increased slowly. This indicates that the types of the two catalysts used in sequence and the timing of adding the catalysts in the present invention have a decisive effect on the intrinsic viscosity and color of the product.

[0126] The above description is merely a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment, it is not intended to limit the present invention. Any technician familiar with the present profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing furandicarboxylic acid polyester, characterized in that: Includes steps: (1) furandicarboxylic acid or furandicarboxylic acid diester and diol undergo esterification or transesterification reaction under the action of a first catalyst, a zinc metal compound, to obtain an esterification or transesterification product P1; (2) P1 is subjected to melt polycondensation reaction at 220-250°C and <50Pa for 2-6 hours to obtain polyester prepolymer P2; (3) Release the vacuum, restore to normal pressure, add the second catalyst or polyester masterbatch P3 containing the second catalyst to P2, the second catalyst is a titanium compound and / or a stannous compound, and mix well; granulate the mixture and pre-crystallize to obtain polyester prepolymer granules P4 containing the second catalyst; Preparation method of P3: add the second catalyst to P2, stir for 5-30 minutes to mix the two, the amount of the second catalyst is 0.3-3wt% of the total mass of furandicarboxylic acid or furandicarboxylic acid diester and diol; (4) solid phase polycondensing P4 at a temperature below its melting point for 3-4 hours in a vacuum or inert gas flow to obtain the product furan dicarboxylic acid polyester; the solid phase polycondensation temperature is gradually increased at a rate of 1-5°C / min so that it is always 5-20°C lower than the melting point of furan dicarboxylic acid polyester.

2. The method for preparing furandicarboxylic acid polyester according to claim 1, characterized in that: The esterification or transesterification reaction in step (1) is carried out at 160-200°C for 2-6 hours.

3. The method for preparing a furandicarboxylic acid polyester according to claim 1 or 2, characterized in that: In step (1), the furandicarboxylic acid is 2,5-furandicarboxylic acid, and the furandicarboxylic acid diester is 2,5-furandicarboxylic acid diester.

4. The method for preparing a furandicarboxylic acid polyester according to claim 1 or 2, characterized in that: The diol in step (1) is selected from at least one of ethylene glycol, propylene glycol and butanediol.

5. The method for preparing furandicarboxylic acid polyester according to claim 1, characterized in that: Step (1) The first catalyst zinc metal compound is selected from one or more of zinc oxide, zinc acetate, zinc lactate, zinc acetylacetonate, zinc citrate and zinc carbonate.

6. The method for preparing furandicarboxylic acid polyester according to claim 5, characterized in that: In step (1), the first catalyst is used in an amount of 0.01-0.2 wt % of the total mass of furandicarboxylic acid or furandicarboxylic acid diester and diol.

7. The method for preparing furandicarboxylic acid polyester according to claim 1, characterized in that: The titanium compound in step (3) is selected from one or more of tetrabutyl titanate, isopropyl titanate, tetraethyl titanate, ethylene glycol titanium, and acetylacetonate titanium.

8. The method for preparing furandicarboxylic acid polyester according to claim 1, characterized in that: The stannous compound in step (3) is selected from one or more of stannous acetate, stannous oxalate, stannous octoate, stannous chloride, stannous bromide and stannous oxide.

9. The method for preparing furandicarboxylic acid polyester according to claim 7 or 8, characterized in that: In step (3), the amount of the second catalyst used is 0.003-0.25 wt % of the total mass of furandicarboxylic acid or furandicarboxylic acid diester and diol.

10. The method for preparing furandicarboxylic acid polyester according to claim 1, characterized in that: The pre-crystallization treatment conditions in step (3) are 70-200 °C for 0.5-6 h.