A high-heat-hardness water-based polyester-modified silicone high-temperature resistant coating and preparation method thereof
By introducing nano-titanium dioxide particles into polyester-modified silicone resin, the problem of polyester-modified silicone high-temperature resistant coatings re-sticking and softening at high temperatures was solved, and a low-VOCs water-based high-temperature resistant coating was developed to achieve high Hardness, self-cleaning and environmentally friendly coating properties.
Patent Information
- Application Number
- CN202211743950.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-30
AI Technical Summary
Existing polyester-modified silicone high-temperature-resistant coatings will stick back, become softer, and reduce hardness under high-temperature conditions, resulting in reduced wear resistance and mechanical properties. At the same time, solvent-based coatings emit organic volatiles during production and use. Threats to the environment and health arise from the lack of industrialized production of water-based high-temperature resistant coatings.
A polyester-modified silicone resin with terminal carboxyl groups of waterable groups is used to perform a neutralization and salt-forming reaction in a water system of modified titanium sol to generate a titanium-containing water-based polyester-modified silicone resin with evenly distributed nano-titanium dioxide particles. , to avoid the adverse effects of external emulsifiers on the coating, and to modify nano-titanium dioxide particles with silane coupling agents to improve compatibility and dispersion stability.
Significantly improves the hardness, heat resistance and water resistance of the coating, protects the ester bonds from hydrolysis and oxidation, gives the coating self-cleaning ability, reduces VOCs emissions, extends service life and improves environmental protection.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new materials, and in particular to a high-heat-hardness water-based polyester-modified organic silicon high-temperature resistant coating and a preparation method thereof. Background Art
[0002] Silicone resin has Si-O bond as the main chain. Since Si-O bond has high bond energy (363kJ / mol) and is relatively stable, it has good heat resistance and is often used to prepare high temperature resistant coatings. However, pure silicone resin has the disadvantages of high curing temperature, long curing time, poor mechanical properties, adhesion and organic solvent resistance of the paint film, and generally needs to be modified. Polyester resin is a polymer made by polycondensation reaction of polyacids and polyols. Each chain segment is connected by ester groups and has good physical and mechanical properties and chemical corrosion resistance. High temperature resistant coatings with polyester modified silicone resin as the main film-forming material have the advantages of excellent heat resistance, adhesion and low surface tension. They can be exposed to open flames, can be used for a long time at 230℃-260℃, and will not change color when baked at 280℃ for 1h. They have been widely used in the external surface coating of various cookers and small household appliances. However, polyester modified silicone high temperature resistant coatings will become sticky and soften under high temperature conditions, and the hardness will decrease, resulting in reduced wear resistance and mechanical properties of the coating, thus affecting its service life.
[0003] In addition, polyester-modified silicone heat-resistant coatings are still mainly solvent-based. Although they have many advantages and market share, the volatile organic compounds (VOCs) emitted during production and construction pose a threat to the environment and people's health. With the increasing awareness of environmental protection and the concept of sustainable development becoming more and more popular, it is a general trend for low-VOCs coatings to replace traditional solvent-based coatings. At present, major coatings companies are accelerating the pace of developing environmentally friendly coatings. In the field of heat-resistant coatings, it is urgent to develop water-based coatings to replace the corresponding solvent-based products. Water-based coatings are a type of coating that uses water as a solvent or dispersion medium. Water replaces the organic solvents in traditional coatings, which significantly reduces the emission of VOCs during production and use. The main film-forming material of water-based heat-resistant coatings, water-based polyester-modified silicone resin, is still in the research and development stage and has not yet entered the stage of large-scale industrial production. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a high thermal hardness water-based polyester-modified silicone high-temperature resistant coating and a preparation method thereof. The present invention causes a polyester-modified silicone resin having a terminal carboxyl group of a water-based group to undergo an in-situ neutralization and salt-forming reaction in the water system of a modified titanium sol to obtain a titanium-containing water-based polyester-modified silicone resin with uniformly distributed nano-titanium dioxide particles, thereby avoiding the adverse effects of externally added emulsifiers on the heat resistance of the final cured coating and the performance degradation and system instability caused by the hydrolysis of ester bonds and the hydrolysis and self-polymerization of incompletely reacted silicone intermediates during the storage of the resin. Nano-titanium dioxide particles can protect the ester bonds from being hydrolyzed and oxidized, so that the coating will not stick back or soften in a heated environment, and still have good hardness; in addition, the nano-titanium dioxide particles also give the coating self-cleaning ability.
[0005] The specific technical scheme of the present invention is:
[0006] In the first aspect, the present invention provides a high thermal hardness water-based polyester-modified silicone high-temperature resistant coating, which is made from the following raw materials in parts by weight: 50-80 parts of polyester-modified silicone resin, 2-6 parts of modified titanium sol, 20-60 parts of high-temperature resistant pigments and fillers, 1-4 parts of additives, 2-4 parts of neutralizers, and 30-80 parts of water.
[0007] The present invention causes a polyester-modified silicone resin having a terminal carboxyl group of a water-soluble group to undergo an in-situ neutralization and salt-forming reaction in a water system of a modified titanium sol (the main component of which is nano-titanium dioxide particles), thereby obtaining a titanium-containing water-based polyester-modified silicone resin in which nano-titanium dioxide particles are uniformly distributed, and can avoid the adverse effects of an externally added emulsifier on the heat resistance of the final cured coating and the problems of performance degradation and system instability caused by the hydrolysis of ester bonds and the hydrolysis and self-polymerization of incompletely reacted silicone intermediates during the storage of the resin. In addition, when the nano-titanium dioxide particles are uniformly distributed in the polyester-modified silicone resin, the hardness, heat resistance and water resistance of the formed coating can be significantly improved, and the ester bonds can be protected from being hydrolyzed and oxidized, so that the coating still has good hardness in a heated environment; at the same time, the nano-titanium dioxide also has excellent ultraviolet shielding, visible light transmittance, antibacterial ability and photocatalytic ability, so that the coating has a certain self-cleaning ability.
[0008] Preferably, the modified titanium sol comprises the following raw materials in parts by weight: 5-10 parts of titanate, 20-40 parts of cosolvent, 10-20 parts of water, 0.1-0.2 parts of acid, and 0.5-1 parts of silane coupling agent.
[0009] Preferably, the preparation method of the modified titanium sol is the following steps: titanate and 50wt% co-solvent are put into a reaction kettle and mixed evenly, the temperature is raised to 60-80°C, water, acid and another 50wt% co-solvent mixture are added dropwise, the reaction is carried out for 1-3h, and then a silane coupling agent is added dropwise, the reaction is continued for 1-2h, and the co-solvent is removed by reduced pressure distillation to obtain a modified titanium sol.
[0010] The modified titanium sol of the present invention is prepared by a sol-gel method, with titanate as a precursor, and hydrolyzed and condensed under the catalysis of an acid to form a titanium sol. The titanium dioxide particles prepared by the method are nanometer-level, and then the nano titanium dioxide particles are organically modified by a silane coupling agent, thereby enhancing the compatibility of the nano titanium dioxide particles with a polyester-modified organic silicone resin, so that the nano titanium dioxide particles have higher dispersion uniformity and dispersion stability in the system.
[0011] Preferably, the titanate is selected from tetrabutyl titanate and tetraisopropyl titanate.
[0012] Preferably, the co-solvent is selected from ethanol and isopropanol.
[0013] Preferably, the acid is selected from hydrochloric acid and acetic acid.
[0014] Preferably, the silane coupling agent is selected from γ-glycidyloxypropyltrimethoxysilane and γ-glycidyloxypropyltriethoxysilane.
[0015] Preferably, the polyester modified silicone resin comprises the following raw materials in parts by weight: 1-5 parts of diol, 10-20 parts of triol, 10-20 parts of dibasic acid, 12-25 parts of silicone intermediate, 3-8 parts of acid anhydride, 0.0005-0.001 parts of catalyst, and 10-20 parts of solvent.
[0016] The polyester-modified silicone resin of the present invention contains terminal carboxyl groups that can be further neutralized to form salts in its molecular structure, and can be made water-based without the need for the addition of an emulsifier, thereby avoiding the adverse effects of the emulsifier on the heat resistance of the final cured coating. In addition, the polyester-modified silicone resin is neutralized to form salts during the preparation of the coating, thereby avoiding the problems of performance degradation and system instability caused by the hydrolysis of ester bonds and the hydrolysis and self-polymerization of incompletely reacted silicone intermediates during the storage of the resin, thereby solving the problems of poor workability and stability of existing water-based polyester-modified silicone resins.
[0017] Preferably, the diol is selected from neopentyl glycol, 1,4-cyclohexanedimethanol, and 1,5-pentanediol.
[0018] Preferably, the triol is selected from trimethylolpropane and trimethylolethane.
[0019] Preferably, the dibasic acid is selected from isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid.
[0020] Preferably, the organosilicon intermediate is phenylmethylpolysiloxane oligomer with a weight average molecular weight of 500-2000 and containing 15-18% methoxy groups; preferably, the organosilicon intermediate is selected from KR510 of Xinyue Company, IC232 of Wacker Company, and DC3074 of Dow Corning Company.
[0021] Preferably, the acid anhydride is selected from trimellitic anhydride and pyromellitic anhydride.
[0022] Preferably, the catalyst is selected from aluminum triacetylacetonate, tetrabutyl titanate, and sodium metaaluminate.
[0023] Preferably, the solvent is selected from dipropylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol methyl ether acetate.
[0024] Preferably, the preparation method of the polyester-modified silicone resin comprises the following steps: adding diol, triol and dibasic acid into a reaction kettle, heating to 170-190°C for esterification for 1-2h, then heating to 210-230°C, continuing the reaction for 2-4h until the acid value drops below 10mgKOH / g, stopping the reaction, cooling to 150-170°C, adding solvent and acid anhydride, continuing the reaction until the acid value reaches 60-80mgKOH / g, cooling to 100-120°C, adding silicone intermediate and catalyst, reacting for 1-2h until transparent, and obtaining the polyester-modified silicone resin.
[0025] The invention uses triol and dibasic acid as monomers to synthesize hyperbranched polyester. Since the polymerization between the two has a gelation tendency, diol is introduced as a central core to regulate the progress of the hyperbranching reaction and better control the molecular weight and molecular weight distribution of the final product. Then, the end capping is performed by an acid anhydride to obtain a carboxyl-hydroxyl-terminated hyperbranched polyester. Then, the hydroxyl groups on the hyperbranched polyester react with the alkoxy groups on the organosilicon intermediate to obtain a polyester-modified organosilicon resin having a water-soluble group carboxyl-terminated group.
[0026] Preferably, the heat-resistant color filler is composed of a mixture of heat-resistant pigments and heat-resistant fillers in any ratio, the pigment is a heat-resistant pigment commonly used in the art, and can be an inorganic heat-resistant pigment such as carbon black and iron red, or an organic heat-resistant pigment such as phthalocyanine green. The filler is a heat-resistant filler commonly used in the art, and can be silicon carbide or aluminum oxide.
[0027] Preferably, the additive includes one or more of a dispersant, a leveling agent, and a defoaming agent; the dispersant is selected from UNIQ-690W and BYK-190; the leveling agent is selected from UNIQ-495U and TEGO-450; the defoaming agent is selected from UNIQ-265W and SURFYNOL-440.
[0028] Preferably, the neutralizing agent is selected from triethylamine, N,N-dimethylethanolamine, and 2-amino-2-methyl-1-propanol.
[0029] In a second aspect, the present invention provides a method for preparing the above-mentioned high thermal hardness water-based polyester-modified silicone high temperature resistant coating, which specifically comprises the following steps:
[0030] (1) Evenly mix the high temperature resistant pigment, filler, additive and water, grind and obtain color paste.
[0031] (2) The polyester modified silicone resin, the modified titanium sol and the neutralizer are mixed evenly, sheared and stirred, and then added to the color paste prepared in step (1) and mixed evenly, and filtered to obtain a high heat hardness water-based polyester modified silicone high temperature resistant coating.
[0032] Compared with the prior art, the present invention has the following technical effects:
[0033] (1) The polyester-modified silicone resin of the present invention is neutralized and salted during the preparation of the coating, thereby avoiding the problems of performance degradation and system instability caused by the hydrolysis of ester bonds and the hydrolysis and self-polymerization of incompletely reacted silicone intermediates during the storage of the resin.
[0034] (2) The present invention organically modifies nano-titanium dioxide particles through a silane coupling agent, thereby enhancing the compatibility of nano-titanium dioxide particles with polyester-modified silicone resin. Using this system as a system, an in-situ neutralization and salt-forming reaction occurs, and the nano-titanium dioxide can be evenly distributed in the resin, which can protect the ester bond from being hydrolyzed and oxidized, so that the coating will not stick back or soften in a heated environment and still have good hardness, and can also give the coating self-cleaning ability; thereby increasing the service life of the coating and facilitating energy saving and consumption reduction.
[0035] (3) The present invention prepares a water-based high-temperature resistant coating by using polyester-modified silicone resin as the main film-forming substance, which greatly reduces VOCs emissions and is an environmentally friendly coating. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with the embodiments.
[0037] Overall embodiment
[0038] A high-heat-hardness water-based polyester-modified silicone high-temperature resistant coating is prepared from the following raw materials in parts by weight:
[0039] 50-80 parts of polyester modified silicone resin, 2-6 parts of modified titanium sol, 20-60 parts of high temperature resistant pigments and fillers, 1-4 parts of additives, 2-4 parts of neutralizers, and 30-80 parts of water.
[0040] The high temperature resistant pigment and filler are composed of a mixture of high temperature resistant pigments and high temperature resistant fillers in any ratio. The pigment is a commonly used high temperature resistant pigment in the art, which can be an inorganic high temperature resistant pigment such as carbon black and iron red, or an organic high temperature resistant pigment such as phthalocyanine green. The filler is a commonly used high temperature resistant filler in the art, which can be silicon carbide or aluminum oxide. The auxiliary agent includes one or more of a dispersant, a leveling agent, and a defoaming agent; the dispersant is selected from UNIQ-690W and BYK-190; the leveling agent is selected from UNIQ-495U and TEGO-450; the defoaming agent is selected from UNIQ-265W and SURFYNOL-440. The neutralizer is selected from triethylamine, N,N-dimethylethanolamine, and 2-amino-2-methyl-1-propanol.
[0041] The preparation method of polyester modified silicone resin comprises the following steps: 1-5 parts (by weight, the same below) of diol, 10-20 parts of triol and 10-20 parts of dibasic acid are put into a reaction kettle, the temperature is raised to 170-190°C for esterification for 1-2 hours, the temperature is then raised to 210-230°C, the reaction is continued for 2-4 hours until the acid value drops below 10 mgKOH / g, the reaction is stopped, the temperature is lowered to 150-170°C, 10-20 parts of solvent and 3-8 parts of acid anhydride are added, the reaction is continued until the acid value reaches 60-80 mgKOH / g, the temperature is lowered to 100-120°C, 12-25 parts of silicone intermediate and 0.0005-0.001 parts of catalyst are added, the reaction is continued for 1-2 hours until transparent, and the polyester modified silicone resin is obtained.
[0042] Among them, the diol is selected from neopentyl glycol, 1,4-cyclohexanedimethanol, and 1,5-pentanediol. The triol is selected from trimethylolpropane and trimethylolethane. The dibasic acid is selected from isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid. The silicone intermediate is selected from KR510 of Xinyue Company, IC232 of Wacker Company, and DC3074 of Dow Corning Company. The anhydride is selected from trimellitic anhydride and pyromellitic anhydride. The catalyst is selected from aluminum triacetylacetonate, tetrabutyl titanate, and sodium aluminate. The solvent is selected from dipropylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol methyl ether acetate.
[0043] The preparation method of the modified titanium sol is as follows: 5-10 parts (by weight, the same below) of titanate and 10-20 parts of a solvent are put into a reaction kettle and mixed evenly, the temperature is raised to 60-80°C, 10-20 parts of water, 0.1-0.2 parts of an acid and another 10-20 parts of a mixture of solvents are added dropwise, the reaction is carried out for 1-3 hours, and then 0.5-1 parts of a silane coupling agent are added dropwise, the reaction is continued for 1-2 hours, and the solvent is removed by reduced pressure distillation to obtain a modified titanium sol.
[0044] Wherein, the titanate is selected from tetrabutyl titanate and tetraisopropyl titanate. The cosolvent is selected from ethanol and isopropanol. The acid is selected from hydrochloric acid and acetic acid. The silane coupling agent is selected from γ-glycidyloxypropyltrimethoxysilane and γ-glycidyloxypropyltriethoxysilane.
[0045] The preparation method of the above-mentioned high thermal hardness water-based polyester modified silicone high temperature resistant coating specifically comprises the following steps:
[0046] (1) Evenly mix the high temperature resistant pigment, additive and water, and grind to a fineness of ≤10 μm to obtain a color paste.
[0047] (2) The polyester modified silicone resin, modified titanium sol and neutralizer are mixed evenly, and stirred at high speed for 1-3 hours, and then added to the color paste prepared in step (1) and mixed evenly, and filtered to obtain a high heat hardness water-based polyester modified silicone high temperature resistant coating.
[0048] Preparation example of polyester modified silicone
[0049] Example 1
[0050] 1 part by weight of neopentyl glycol, 10 parts by weight of trimethylolpropane and 10 parts by weight of isophthalic acid were put into a reactor, the temperature was raised to 170°C and kept for esterification for 2 hours, then the temperature was raised to 210°C and the reaction was continued for 4 hours until the acid value dropped to 8.6 mgKOH / g, the reaction was stopped, the temperature was lowered to 150°C, 10 parts by weight of ethylene glycol butyl ether and 3 parts by weight of trimellitic anhydride were added, the reaction was continued until the acid value was 69.2 mgKOH / g, the temperature was lowered to 100°C, 12 parts by weight of organosilicon intermediate DC3074 and 0.0005 parts by weight of tetrabutyl titanate were added, the reaction was continued for 2 hours until transparent, and a polyester modified organosilicon resin was obtained.
[0051] Example 2
[0052] 5 parts by weight of 1,4-cyclohexanedimethanol, 20 parts by weight of trimethylolethane and 20 parts by weight of 1,4-cyclohexanedicarboxylic acid were put into a reactor, the temperature was raised to 190°C and kept for esterification for 1 hour, then the temperature was raised to 230°C, the reaction was continued for 2 hours until the acid value dropped to 9.4 mgKOH / g, the reaction was stopped, the temperature was lowered to 170°C, 20 parts by weight of propylene glycol methyl ether acetate and 8 parts by weight of pyromellitic anhydride were added, the reaction was continued until the acid value was 71.5 mgKOH / g, the temperature was lowered to 120°C, 25 parts by weight of silicone intermediate IC232 and 0.001 parts by weight of aluminum triacetylacetonate were added, the reaction was continued for 1 hour until transparent, and a polyester modified silicone resin was obtained.
[0053] Example 3
[0054] 2 parts by weight of 1,5-pentanediol, 15 parts by weight of trimethylolpropane and 18 parts by weight of terephthalic acid were put into a reactor, the temperature was raised to 180°C and kept for esterification for 1.5 hours, then the temperature was raised to 220°C, the reaction was continued for 3 hours until the acid value dropped to 9.5 mgKOH / g, the reaction was stopped, the temperature was lowered to 160°C, 15 parts by weight of dipropylene glycol methyl ether and 5 parts by weight of trimellitic anhydride were added, the reaction was continued until the acid value was 70.8 mgKOH / g, the temperature was lowered to 110°C, 20 parts by weight of silicone intermediate KR510 and 0.0008 parts by weight of sodium aluminate were added, the reaction was continued for 1.5 hours until transparent, and a polyester modified silicone resin was obtained.
[0055] Preparation example of modified titanium sol
[0056] Example 4
[0057] 5 parts by weight of tetrabutyl titanate and 10 parts by weight of ethanol were put into a reaction kettle and mixed evenly. The temperature was raised to 60°C, and a mixture of 10 parts by weight of water, 0.1 parts by weight of hydrochloric acid and 10 parts by weight of ethanol was added dropwise. The reaction was continued for 3 hours. Then, 0.5 parts by weight of γ-glycidyloxypropyltrimethoxysilane was added dropwise. The reaction was continued for 2 hours. The co-solvent was removed by distillation under reduced pressure to obtain a modified titanium sol.
[0058] Example 5
[0059] 10 parts by weight of tetraisopropyl titanate and 20 parts by weight of isopropanol were put into a reaction kettle and mixed evenly, the temperature was raised to 80°C, 20 parts by weight of water, 0.2 parts by weight of acetic acid and another 20 parts by weight of isopropanol were added dropwise, the reaction was continued for 1 hour, and then 1 part by weight of γ-glycidyloxypropyltriethoxysilane was added dropwise, the reaction was continued for 1 hour, and the co-solvent was removed by distillation under reduced pressure to obtain a modified titanium sol.
[0060] Coating Preparation Example
[0061] Example 6
[0062] (1) 5 parts by weight of carbon black, 15 parts by weight of silicon carbide, 0.7 parts by weight of UNIQ-690W, 0.3 parts by weight of UNIQ-495U, and 30 parts by weight of water were mixed and evenly ground to a fineness of ≤10 μm to obtain a black color paste.
[0063] (2) 50 parts by weight of the polyester modified silicone resin prepared in Example 1, 2 parts by weight of the modified titanium sol prepared in Example 4, and 2 parts by weight of N,N-dimethylethanolamine are mixed evenly, and stirred at high speed for 1 hour. Then, the mixture is added to the black color paste prepared in step (1) and mixed evenly. The mixture is filtered to obtain a high heat hardness water-based polyester modified silicone high temperature resistant coating.
[0064] Example 7
[0065] (1) 20 parts by weight of iron oxide red, 40 parts by weight of aluminum oxide, 2 parts by weight of BYK-190, 1 part by weight of TEGO-450, 1 part by weight of UNIQ-265W, and 80 parts by weight of water were mixed and evenly ground to a fineness of ≤10 μm to obtain a red color paste.
[0066] (2) 80 parts by weight of the polyester modified silicone resin prepared in Example 2, 6 parts by weight of the modified titanium sol prepared in Example 5, and 4 parts by weight of triethylamine are mixed evenly, stirred at high speed for 3 hours, and then added to the red color paste prepared in step (1) and mixed evenly. Filter to obtain a high thermal hardness water-based polyester modified silicone high temperature resistant coating.
[0067] Example 8
[0068] (1) 15 parts by weight of phthalocyanine green, 25 parts by weight of aluminum oxide, 2 parts by weight of UNIQ-690W, 0.7 parts by weight of UNIQ-495U, 0.3 parts by weight of SURFYNOL-440 additive, and 60 parts by weight of water were mixed and evenly ground to a fineness of ≤10 μm to obtain a green color paste.
[0069] (2) 60 parts by weight of the polyester modified silicone resin prepared in Example 3, 5 parts by weight of the modified titanium sol prepared in Example 4, and 3 parts by weight of 2-amino-2-methyl-1-propanol are mixed evenly, stirred at high speed for 2 hours, and then added to the green color paste prepared in step (1) and mixed evenly. Filter to obtain a high thermal hardness water-based polyester modified silicone high temperature resistant coating.
[0070] Comparative Example 1
[0071] The only difference from Example 6 is that no modified titanium sol is added in step (2), and the remaining steps as well as materials and compositions are consistent with Example 6.
[0072] Comparative Example 2
[0073] The only difference from Example 6 is that in step (2), modified titanium sol is not added, but is replaced by unmodified titanium sol of the same weight portion, and the remaining steps, materials and composition are consistent with Example 6.
[0074] Comparative Example 3
[0075] The only difference from Example 6 is that in step (2), the polyester-modified silicone resin is first neutralized with N,N-dimethylethanolamine and water and then added. The remaining steps, materials and compositions are consistent with Example 6.
[0076] Performance Testing
[0077] The high heat hardness water-based polyester modified silicone high temperature resistant coatings prepared in Examples 6-8 and the coatings prepared in Comparative Examples 1-3 were coated on aluminum substrates (the coating thickness was controlled to be 15 μm), and then the hardness, adhesion, heat resistance, hot hardness, self-cleaning and anti-fouling properties and other properties were tested, wherein the hardness test was carried out according to the provisions of GB / T 6739, and the result evaluation was: the paint film was scratched; the adhesion test was carried out according to the provisions of GB / T 9286, with a spacing of 1 mm; the heat resistance was measured according to the standard of GB / T 1735, and the test conditions were: 280°C*30min, and the result evaluation was: the color difference ≤1 was qualified; the hot hardness test, the coated substrate was placed in a 150°C oven, and then the hardness was measured according to the provisions of GB / T 6739; the self-cleaning and anti-fouling test was carried out by staining the coating with oil pen stains, then scrubbing, repeating 50 times, and it was qualified if it could be completely erased. The test results are shown in Table 1.
[0078] Table 1 Product performance test results of Examples 6-8 and Comparative Examples 1-3:
[0079] hardness Adhesion Heat resistance Hot hardness Self-cleaning and anti-fouling Example 6 3H Level 0 qualified 2H qualified Example 7 3H Level 0 qualified 2H qualified Example 8 3H Level 0 qualified 2H qualified Comparative Example 1 2H Level 0 qualified B Failure Comparative Example 2 3H Level 1 qualified B Failure Comparative Example 3 3H Level 0 qualified H Failure
[0080] From the above data comparison, we can see that:
[0081] In Comparative Example 1, no modified titanium sol is added, and the hardness of the water-based polyester modified silicone coating decreases, and a good thermal hardness cannot be maintained. In a heated environment, the coating is damaged, and the self-cleaning and anti-fouling properties are unqualified.
[0082] Comparative Example 2 adds unmodified titanium sol, which has poor compatibility with polyester-modified silicone, uneven coating, reduced adhesion, and although the initial hardness is improved, the thermal hardness decreases significantly after heating, and the coating does not have good self-cleaning and anti-fouling properties.
[0083] The polyester-modified silicone resin added in Comparative Example 3 has been neutralized and made aqueous before being added. The uniform dispersion of the nano-titanium dioxide particles is limited, the initial hardness and thermal hardness are acceptable, but the self-cleaning and anti-fouling properties are unsatisfactory. In addition, the storage stability of the aqueous polyester-modified silicone resin is poor, which will lead to a decrease in performance.
[0084] Compared with comparative examples 1-3, the high thermal hardness water-based polyester modified silicone high temperature resistant coatings of Examples 6-8 have nano-titanium dioxide that can be evenly distributed in the resin, which can protect the ester bonds from hydrolysis and oxidation, prevent the coating from sticking back and softening in a heated environment, and have good thermal hardness, and can also give the coating self-cleaning ability.
[0085] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0086] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for improving the thermal hardness of a water-based polyester modified silicone high temperature resistant coating after film formation, characterized in that The steps include: (1) 5-10 parts of titanate and 10-20 parts of co-solvent are put into a reaction kettle and mixed evenly, the temperature is raised, and a mixture of 10-20 parts of water, 0.1-0.2 parts of acid and another 10-20 parts of co-solvent is added dropwise, and the mixture is reacted at 60-80° C. for 1-3 hours; then 0.5-1 parts of silane coupling agent is added dropwise, the reaction is continued for 1-2 hours, and the co-solvent is removed by reduced pressure distillation to obtain a modified titanium sol; (2) Mix 20-60 parts of high temperature resistant pigments and fillers, 1-4 parts of additives, and 30-80 parts of water, and grind to obtain a color paste; (3) Mix 50-80 parts of polyester modified silicone resin with terminal carboxyl groups, 2-6 parts of modified titanium sol, and 1-4 parts of neutralizer, shear and stir, add to the color paste, mix, filter, and obtain a high heat hardness water-based polyester modified silicone high temperature resistant coating; The polyester modified silicone resin includes the following raw materials: 1-5 parts of diol, 10-20 parts of triol, 10-20 parts of dibasic acid, 12-25 parts of silicone intermediate, 3-8 parts of acid anhydride, 0.0005-0.001 parts of catalyst, and 10-20 parts of solvent; The neutralizing agent is selected from triethylamine, N,N-dimethylethanolamine, and 2-amino-2-methyl-1-propanol; The above parts are all parts by weight.
2. The method according to claim 1, characterized in that: In step (1), The titanate is selected from tetrabutyl titanate and tetraisopropyl titanate; The silane coupling agent is selected from γ-glycidyloxypropyltrimethoxysilane and γ-glycidyloxypropyltriethoxysilane; The cosolvent is selected from ethanol and isopropanol; The acid is selected from hydrochloric acid and acetic acid.
3. The method according to claim 1, characterized in that: The preparation method of the polyester modified silicone resin comprises: putting 1-5 parts by weight of diol, 10-20 parts by weight of triol and 10-20 parts by weight of dibasic acid into a reaction kettle, heating to 170-190° C. for esterification for 1-2 hours, then heating to 210-230° C., continuing to react for 2-4 hours until the acid value drops below 10 mgKOH / g, stopping the reaction, cooling to 150-170° C., adding 10-20 parts by weight of solvent and 3-8 parts by weight of acid anhydride, continuing to react until the acid value reaches 60-80 mgKOH / g, cooling to 100-120° C., adding 12-25 parts by weight of silicone intermediate and 0.0005-0.001 parts by weight of catalyst, reacting for 1-2 hours until transparent, and preparing the polyester modified silicone resin.
4. The method according to claim 1, characterized in that: The diol is selected from neopentyl glycol, 1,4-cyclohexanedimethanol, and 1,5-pentanediol; The triol is selected from trimethylolpropane and trimethylolethane; The dibasic acid is selected from isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid; The acid anhydride is selected from trimellitic anhydride and pyromellitic anhydride; The organosilicon intermediate is a phenylmethyl polysiloxane oligomer with a weight average molecular weight of 500-2000 and containing 15-18% methoxy groups; The catalyst is selected from aluminum triacetylacetonate, tetrabutyl titanate, and sodium metaaluminate; The solvent is selected from dipropylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol methyl ether acetate.
5. The method according to claim 1, characterized in that: The auxiliary agent includes one or more of a dispersant, a leveling agent, and a defoaming agent.
6. The application of modified titanium sol in improving the thermal hardness of waterborne polyester modified silicone high temperature resistant coating after film formation, characterized in that: The preparation of the modified titanium sol comprises: (1) 5-10 parts of titanate and 10-20 parts of co-solvent are put into a reaction kettle and mixed evenly, the temperature is raised, and a mixture of 10-20 parts of water, 0.1-0.2 parts of acid and another 10-20 parts of co-solvent is added dropwise, and the mixture is reacted at 60-80° C. for 1-3 hours; then 0.5-1 parts of silane coupling agent is added dropwise, the reaction is continued for 1-2 hours, and the co-solvent is removed by reduced pressure distillation to obtain a modified titanium sol; The preparation of the waterborne polyester modified silicone high temperature resistant coating comprises: (2) Mix 20-60 parts of high temperature resistant pigments and fillers, 1-4 parts of additives, and 30-80 parts of water, and grind to obtain a color paste; (3) Mix 50-80 parts of polyester modified silicone resin with terminal carboxyl groups, 2-6 parts of modified titanium sol, and 1-4 parts of neutralizer, shear and stir, add to the color paste, mix, filter, and obtain a high heat hardness water-based polyester modified silicone high temperature resistant coating; The polyester modified silicone resin includes the following raw materials: 1-5 parts of diol, 10-20 parts of triol, 10-20 parts of dibasic acid, 12-25 parts of silicone intermediate, 3-8 parts of acid anhydride, 0.0005-0.001 parts of catalyst, and 10-20 parts of solvent; The neutralizing agent is selected from triethylamine, N,N-dimethylethanolamine, and 2-amino-2-methyl-1-propanol; the above parts are all parts by weight.
7. The use according to claim 6, characterized in that: In step (1), The titanate is selected from tetrabutyl titanate and tetraisopropyl titanate; The silane coupling agent is selected from γ-glycidyloxypropyltrimethoxysilane and γ-glycidyloxypropyltriethoxysilane; The cosolvent is selected from ethanol and isopropanol; The acid is selected from hydrochloric acid and acetic acid.
8. The use according to claim 6, characterized in that: The preparation method of the polyester modified silicone resin comprises: putting 1-5 parts by weight of diol, 10-20 parts by weight of triol and 10-20 parts by weight of dibasic acid into a reaction kettle, heating to 170-190° C. for esterification for 1-2 hours, then heating to 210-230° C., continuing to react for 2-4 hours until the acid value drops below 10 mgKOH / g, stopping the reaction, cooling to 150-170° C., adding 10-20 parts by weight of solvent and 3-8 parts by weight of acid anhydride, continuing to react until the acid value reaches 60-80 mgKOH / g, cooling to 100-120° C., adding 12-25 parts by weight of silicone intermediate and 0.0005-0.001 parts by weight of catalyst, reacting for 1-2 hours until transparent, and preparing the polyester modified silicone resin.
9. The use according to claim 6, characterized in that: The diol is selected from neopentyl glycol, 1,4-cyclohexanedimethanol, and 1,5-pentanediol; The triol is selected from trimethylolpropane and trimethylolethane; The dibasic acid is selected from isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid; The acid anhydride is selected from trimellitic anhydride and pyromellitic anhydride; The organosilicon intermediate is a phenylmethyl polysiloxane oligomer with a weight average molecular weight of 500-2000 and containing 15-18% methoxy groups; The catalyst is selected from aluminum triacetylacetonate, tetrabutyl titanate, and sodium metaaluminate; The solvent is selected from dipropylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol methyl ether acetate.