A BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst and its preparation method and application

Through the BiFeO3/Bi2WO6 two-dimensional single crystal heterojunction structure, the problem of visible light response and recycling of bismuth tungstate photocatalyst is solved, and efficient photocatalytic performance and rapid degradation effect are achieved.

CN116273039BActive Publication Date: 2024-10-18YUNNAN NORMAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310312815.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-18
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Existing bismuth tungstate photocatalysts are unsatisfactory in the visible light response region, have low electron transport performance, and their tightly stacked structure results in a small specific surface area, which affects the photocatalytic efficiency and is difficult to recycle.

Method used

By compounding with BiFeO3, using a two-dimensional single crystal heterojunction structure, and using hydrothermal treatment to prepare BiFeO3/Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, bismuth tungstate is spaced on the bismuth ferrite single crystal nanosheets, growing vertically, improving Specific surface area and carrier separation efficiency, and utilize the magnetism of bismuth ferrite to facilitate recycling.

Benefits of technology

The photocatalytic performance and degradation efficiency of bismuth tungstate are significantly improved, and it can quickly degrade methylene blue and rhodamine under visible light, solving the recycling problem and maintaining efficient catalyst recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116273039B_ABST
    Figure CN116273039B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, comprising the following preparation steps: 1) preparing a suspension containing bismuth and tungsten hydroxide oxide precipitation; 2) transferring the suspension prepared in step 1) to a reactor inner tank, adjusting the volume of the suspension in the reactor inner tank to 70% to 90% of the volume of the reactor inner tank with deionized water, stirring evenly, and obtaining a mixed solution; 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly, and obtaining a reaction material; 4) placing the reactor inner tank configured with the reaction material in step 3) in a reactor, sealing it, and performing hydrothermal treatment at 150 to 200° C. for 4.5 to 24 hours; 5) after the hydrothermal reaction is completed, allowing the reactor to cool naturally to room temperature, repeatedly washing the reaction product with deionized water and anhydrous ethanol, filtering, and drying, and obtaining the BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of two-dimensional composite materials, and in particular to a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst and a preparation method and application thereof. Background Art

[0002] Orthogonal bismuth tungstate (Bi2WO6, BWO) is one of the most promising catalysts in visible light photocatalysts and a research hotspot in the field of catalysis. It has good photocatalytic performance. However, in practical applications, people are not satisfied with the visible light response region of bismuth tungstate (≤450nm), its electron transport performance is low, and the photogenerated electron-hole recombination rate is very fast. From the perspective of material structure, firstly, the nano bismuth tungstate material is too small and it is difficult to recycle after the photocatalytic reaction; secondly, bismuth tungstate is a layered material, and its morphology is easily affected by the conditions during synthesis, and it is easy to form spherical flower-shaped, lamellar, and block-shaped sheets; this tightly stacked structure will greatly reduce its specific surface area, thereby affecting the photocatalytic efficiency of bismuth tungstate. Therefore, improving the photocatalytic efficiency of bismuth tungstate and solving the problem of recycling have become the focus of attention.

[0003] Modifying catalysts by composite interface has been proven to be an effective method. In particular, photocatalytic materials based on heterojunctions or interfaces show obvious advantages in photocatalytic performance compared with single-phase photocatalytic materials. The main reason for the improvement is that the lattice and energy band positions at the interface match each other, effectively separating photogenerated electrons and photogenerated holes. BiFeO3 (BFO) has a smaller bandgap (2.0-2.8eV) and has certain advantages in photocatalysis. First, it has a wide light absorption range. After the bismuth ferrite and bismuth tungstate nanomaterials are composited, the efficiency of the bismuth tungstate photocatalytic reaction can be improved, which is beneficial to improve the selectivity of photocatalytic degradation of organic matter. Second, bismuth ferrite is magnetic and easy to recycle, which effectively solves the application problem of improving the recycling and reuse of catalysts. Third, both bismuth ferrite and bismuth tungstate contain bismuth elements. Bismuth tungstate can be epitaxially grown on bismuth ferrite substrates. After composite, a special interface structure may be obtained to improve the separation efficiency of carriers and solve the problem of small specific surface area after bismuth tungstate growth and stacking. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst and a preparation method and application thereof.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] A method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst comprises the following preparation steps:

[0007] 1) preparing a suspension containing bismuth and tungsten oxyhydroxide precipitates;

[0008] 2) transferring the suspension prepared in step 1) into the inner tank of a reaction kettle, adjusting the volume of the suspension in the inner tank of the reaction kettle to 70-90% of the volume of the inner tank of the reaction kettle with deionized water, and stirring evenly to obtain a mixed solution;

[0009] 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly to obtain a reaction material;

[0010] 4) placing the reaction vessel liner containing the reaction materials in step 3) in the reaction vessel, sealing it, and performing hydrothermal treatment at 150-200° C. for 4.5-24 hours;

[0011] 5) After the hydrothermal reaction is completed, the reactor is allowed to cool naturally to room temperature, and the reaction product is repeatedly washed with deionized water and anhydrous ethanol, filtered, and dried to obtain a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst;

[0012] In the step 1), the preparation steps of the suspension containing bismuth and tungsten oxyhydroxide precipitates are:

[0013] S1: prepare bismuth nitrate-dilute nitric acid solution; prepare sodium tungstate aqueous solution;

[0014] S2: Mix the two solutions prepared in S1 and stir them evenly to obtain a mixed solution;

[0015] S3: adding potassium hydroxide aqueous solution to the mixed solution prepared in S2, adjusting the solution pH to 6, and fully stirring at room temperature to obtain a suspension containing bismuth and tungsten hydroxide oxide precipitates;

[0016] The specific steps of step S1 are: weighing bismuth nitrate and sodium tungstate in a molar ratio of 2:1, dissolving bismuth nitrate in 15% dilute nitric acid to obtain a bismuth nitrate-dilute nitric acid solution; dissolving sodium tungstate in deionized water to obtain a sodium tungstate aqueous solution;

[0017] The molar ratio of sodium tungstate to bismuth ferrite is 0.05-0.2:1;

[0018] The present invention also provides a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, which is prepared by the above method, wherein bismuth tungstate can be distributed at intervals on bismuth ferrite single crystal nanosheets and present a sheet structure growth perpendicular to the bismuth ferrite.

[0019] The above-mentioned BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst is used to catalytically degrade methylene blue and rhodamine under visible light.

[0020] Perovskite phase bismuth ferrite single crystal nanosheets can be prepared by the method authorized by Chinese patent CN102877130B.

[0021] The present invention has the following advantages:

[0022] 1. During the implementation of the process of the present invention, no other impurity ions are introduced, and only deionized water and ethanol need to be used for washing after the hydrothermal reaction;

[0023] 2. A BiFeO3 / Bi2WO6 single crystal heterojunction with a special structure was prepared by hydrothermal reaction. Since the lattices of bismuth ferrite and bismuth tungstate can match, bismuth tungstate can be distributed on the bismuth ferrite single crystal nanosheets at intervals and grow in a sheet structure perpendicular to bismuth ferrite, rather than the common multi-layer bismuth tungstate nanosheets stacked together. Such morphological characteristics make bismuth tungstate have a larger specific surface area, thereby further improving the catalytic efficiency;

[0024] 3. After bismuth ferrite and bismuth tungstate are combined, photogenerated electrons and photogenerated holes are effectively separated, the separation efficiency of carriers is improved, and thus the photocatalytic performance is improved; on the other hand, bismuth ferrite particles are large, have weak magnetism, and are easy to recycle, which can effectively solve the application problem of improving the recycling and reuse of bismuth tungstate catalysts;

[0025] 4. The BiFeO3 / Bi2WO6 single crystal heterojunction photocatalyst prepared by the present invention can degrade 92% of methylene blue (MB) within 5 hours under visible light and degrade 60% of rhodamine B within 8 hours under visible light. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 a is the X-ray diffraction (XRD) pattern of the BiFeO3 / Bi2WO6 single crystal heterojunction prepared by the present invention.

[0027] Figure 1 b is a scanning electron microscope (SEM) photograph of the BiFeO3 / Bi2WO6 single crystal heterojunction prepared by the present invention.

[0028] Figure 2 It is the UV-visible light absorption diagram of the BiFeO3 / Bi2WO6 single crystal heterojunction prepared by the present invention when degrading methylene blue (MB) at different times.

[0029] Figure 3 It is the ultraviolet-visible light absorption diagram of the BiFeO3 / Bi2WO6 single crystal heterojunction prepared by the present invention degrading Rhodamine B at different times. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0031] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0033] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0034] Example 1: A method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, comprising the following preparation steps:

[0035] 1) preparing a suspension containing bismuth and tungsten oxyhydroxide precipitates;

[0036] 2) transferring the suspension prepared in step 1) into the inner tank of a reaction kettle, adjusting the volume of the suspension in the inner tank of the reaction kettle to 70-90% of the volume of the inner tank of the reaction kettle with deionized water, and stirring evenly to obtain a mixed solution;

[0037] 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly to obtain a reaction material;

[0038] 4) placing the reaction vessel liner containing the reaction materials in step 3) in the reaction vessel, sealing it, and performing hydrothermal treatment at 150-200° C. for 4.5-24 hours;

[0039] 5) After the hydrothermal reaction is completed, the reactor is allowed to cool naturally to room temperature, and the reaction product is repeatedly washed with deionized water and anhydrous ethanol, filtered, and dried to obtain a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction.

[0040] In the step 1), the preparation steps of the suspension containing bismuth and tungsten oxyhydroxide precipitates are:

[0041] S1: prepare bismuth nitrate-dilute nitric acid solution; prepare sodium tungstate aqueous solution;

[0042] S2: Mix the two solutions prepared in S1 and stir them evenly to obtain a mixed solution;

[0043] S3: adding potassium hydroxide aqueous solution to the mixed solution prepared in S2, adjusting the solution pH to 6, and fully stirring at room temperature to obtain a suspension containing bismuth and tungsten hydroxide oxide precipitates.

[0044] The specific steps of step S1 are: weighing bismuth nitrate and sodium tungstate in a molar ratio of 2:1, dissolving bismuth nitrate in 15% dilute nitric acid to obtain a bismuth nitrate-dilute nitric acid solution; and dissolving sodium tungstate in deionized water to obtain a sodium tungstate aqueous solution.

[0045] The molar ratio of the sodium tungstate to the bismuth ferrite is 0.05-0.2:1.

[0046] from Figure 1 In the XRD spectrum shown in a, the diffraction peaks of bismuth ferrite and bismuth tungstate can be clearly observed, proving that the material contains bismuth ferrite and bismuth tungstate.

[0047] from Figure 1 In the SEM image shown in b, it can be clearly observed that bismuth tungstate is distributed at intervals on the single crystal bismuth ferrite micro-nanosheets, and grows in a sheet-like structure perpendicular to the bismuth ferrite, rather than the common morphology of multi-layer bismuth tungstate nanosheets stacked together.

[0048] Example 2: A method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, comprising the following preparation steps:

[0049] 1) preparing a suspension containing bismuth and tungsten oxyhydroxide precipitates;

[0050] 2) transferring the suspension prepared in step 1) into the inner tank of a reaction kettle, adjusting the volume of the suspension in the inner tank of the reaction kettle to 80% of the volume of the inner tank of the reaction kettle with deionized water, and stirring evenly to obtain a mixed solution;

[0051] 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly to obtain a reaction material;

[0052] 4) placing the reactor liner containing the reaction materials in step 3) in the reactor, sealing it, and performing hydrothermal treatment at 180° C. for 4.5 h;

[0053] 5) After the hydrothermal reaction is completed, the reactor is allowed to cool naturally to room temperature, and the reaction product is repeatedly washed with deionized water and anhydrous ethanol, filtered, and dried to obtain a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction.

[0054] In the step 1), the preparation steps of the suspension containing bismuth and tungsten oxyhydroxide precipitates are:

[0055] S1: prepare bismuth nitrate-dilute nitric acid solution; prepare sodium tungstate aqueous solution;

[0056] S2: Mix the two solutions prepared in S1 and stir them evenly to obtain a mixed solution;

[0057] S3: adding potassium hydroxide aqueous solution to the mixed solution prepared in S2, adjusting the solution pH to 6, and fully stirring at room temperature to obtain a suspension containing bismuth and tungsten hydroxide oxide precipitates.

[0058] The specific steps of step S1 are: weighing bismuth nitrate and sodium tungstate in a molar ratio of 2:1, dissolving bismuth nitrate in 15% dilute nitric acid to obtain a bismuth nitrate-dilute nitric acid solution; and dissolving sodium tungstate in deionized water to obtain a sodium tungstate aqueous solution.

[0059] The molar ratio of sodium tungstate to bismuth ferrite is 0.15:1.

[0060] Example 3: A method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, comprising the following preparation steps:

[0061] 1) preparing a suspension containing bismuth and tungsten oxyhydroxide precipitates;

[0062] 2) transferring the suspension prepared in step 1) into the inner tank of a reaction kettle, adjusting the volume of the suspension in the inner tank of the reaction kettle to 75% of the volume of the inner tank of the reaction kettle with deionized water, and stirring evenly to obtain a mixed solution;

[0063] 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly to obtain a reaction material;

[0064] 4) placing the reactor liner containing the reaction materials in step 3) in the reactor, sealing it, and performing hydrothermal treatment at 180° C. for 6 h;

[0065] 5) After the hydrothermal reaction is completed, the reactor is allowed to cool naturally to room temperature, and the reaction product is repeatedly washed with deionized water and anhydrous ethanol, filtered, and dried to obtain a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction.

[0066] In the step 1), the preparation steps of the suspension containing bismuth and tungsten oxyhydroxide precipitates are:

[0067] S1: prepare bismuth nitrate-dilute nitric acid solution; prepare sodium tungstate aqueous solution;

[0068] S2: Mix the two solutions prepared in S1 and stir them evenly to obtain a mixed solution;

[0069] S3: adding potassium hydroxide aqueous solution to the mixed solution prepared in S2, adjusting the solution pH to 6, and stirring sufficiently to obtain a suspension containing bismuth and tungsten hydroxide oxide precipitates.

[0070] The specific steps of step S1 are: weighing bismuth nitrate and sodium tungstate in a molar ratio of 2:1, dissolving bismuth nitrate in 15% dilute nitric acid to obtain a bismuth nitrate-dilute nitric acid solution; and dissolving sodium tungstate in deionized water to obtain a sodium tungstate aqueous solution.

[0071] The molar ratio of sodium tungstate to bismuth ferrite is 0.05:1.

[0072] Example 4: A method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, comprising the following preparation steps:

[0073] 1) preparing a suspension containing bismuth and tungsten oxyhydroxide precipitates;

[0074] 2) transferring the suspension prepared in step 1) into the inner tank of a reaction kettle, adjusting the volume of the suspension in the inner tank of the reaction kettle to 85% of the volume of the inner tank of the reaction kettle with deionized water, and stirring evenly to obtain a mixed solution;

[0075] 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly to obtain a reaction material;

[0076] 4) placing the reactor liner containing the reaction materials in step 3) in the reactor, sealing it, and performing hydrothermal treatment at 180° C. for 4.5 h;

[0077] 5) After the hydrothermal reaction is completed, the reactor is allowed to cool naturally to room temperature, and the reaction product is repeatedly washed with deionized water and anhydrous ethanol, filtered, and dried to obtain a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction.

[0078] In the step 1), the preparation steps of the suspension containing bismuth and tungsten oxyhydroxide precipitates are:

[0079] S1: prepare bismuth nitrate-dilute nitric acid solution; prepare sodium tungstate aqueous solution;

[0080] S2: Mix the two solutions prepared in S1 and stir them evenly to obtain a mixed solution;

[0081] S3: adding potassium hydroxide aqueous solution to the mixed solution prepared in S2, adjusting the solution pH to 6, and stirring sufficiently to obtain a suspension containing bismuth and tungsten hydroxide oxide precipitates.

[0082] The specific steps of step S1 are: weighing bismuth nitrate and sodium tungstate in a molar ratio of 2:1, dissolving bismuth nitrate in 15% dilute nitric acid to obtain a bismuth nitrate-dilute nitric acid solution; and dissolving sodium tungstate in deionized water to obtain a sodium tungstate aqueous solution.

[0083] The molar ratio of sodium tungstate to bismuth ferrite is 0.1:1.

[0084] Example 5: A method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, comprising the following preparation steps:

[0085] 1) preparing a suspension containing bismuth and tungsten oxyhydroxide precipitates;

[0086] 2) transferring the suspension prepared in step 1) into the inner tank of a reaction kettle, adjusting the volume of the suspension in the inner tank of the reaction kettle to 70% of the volume of the inner tank of the reaction kettle with deionized water, and stirring evenly to obtain a mixed solution;

[0087] 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly to obtain a reaction material;

[0088] 4) placing the reactor liner containing the reaction materials in step 3) in the reactor, sealing it, and performing hydrothermal treatment at 150° C. for 4.5 h;

[0089] 5) After the hydrothermal reaction is completed, the reactor is allowed to cool naturally to room temperature, and the reaction product is repeatedly washed with deionized water and anhydrous ethanol, filtered, and dried to obtain a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction.

[0090] In the step 1), the preparation steps of the suspension containing bismuth and tungsten oxyhydroxide precipitates are:

[0091] S1: prepare bismuth nitrate-dilute nitric acid solution; prepare sodium tungstate aqueous solution;

[0092] S2: Mix the two solutions prepared in S1 and stir them evenly to obtain a mixed solution;

[0093] S3: adding potassium hydroxide aqueous solution to the mixed solution prepared in S2, adjusting the solution pH to 6, and stirring sufficiently to obtain a suspension containing bismuth and tungsten hydroxide oxide precipitates.

[0094] The specific steps of step S1 are: weighing bismuth nitrate and sodium tungstate in a molar ratio of 2:1, dissolving bismuth nitrate in 15% dilute nitric acid to obtain a bismuth nitrate-dilute nitric acid solution; and dissolving sodium tungstate in deionized water to obtain a sodium tungstate aqueous solution.

[0095] The molar ratio of sodium tungstate to bismuth ferrite is 0.05:1.

[0096] Example 6: A method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, comprising the following preparation steps:

[0097] 1) preparing a suspension containing bismuth and tungsten oxyhydroxide precipitates;

[0098] 2) transferring the suspension prepared in step 1) into the inner tank of a reaction kettle, adjusting the volume of the suspension in the inner tank of the reaction kettle to 90% of the volume of the inner tank of the reaction kettle with deionized water, and stirring evenly to obtain a mixed solution;

[0099] 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly to obtain a reaction material;

[0100] 4) placing the reactor liner containing the reaction materials in step 3) in the reactor, sealing it, and performing hydrothermal treatment at 200° C. for 24 hours;

[0101] 5) After the hydrothermal reaction is completed, the reactor is allowed to cool naturally to room temperature, and the reaction product is repeatedly washed with deionized water and anhydrous ethanol, filtered, and dried to obtain a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction.

[0102] In the step 1), the preparation steps of the suspension containing bismuth and tungsten oxyhydroxide precipitates are:

[0103] S1: prepare bismuth nitrate-dilute nitric acid solution; prepare sodium tungstate aqueous solution;

[0104] S2: Mix the two solutions prepared in S1 and stir them evenly to obtain a mixed solution;

[0105] S3: adding potassium hydroxide aqueous solution to the mixed solution prepared in S2, adjusting the solution pH to 6, and stirring sufficiently to obtain a suspension containing bismuth and tungsten hydroxide oxide precipitates.

[0106] The specific steps of step S1 are: weighing bismuth nitrate and sodium tungstate in a molar ratio of 2:1, dissolving bismuth nitrate in 15% dilute nitric acid to obtain a bismuth nitrate-dilute nitric acid solution; and dissolving sodium tungstate in deionized water to obtain a sodium tungstate aqueous solution.

[0107] The molar ratio of sodium tungstate to bismuth ferrite is 0.2:1.

[0108] Example 7: Photocatalytic degradation experiment

[0109] Catalytic degradation of methylene blue solution experiment: The catalyst dosage is 0.1g per 100ml of methylene blue solution, and the concentration of methylene blue solution is 10 -5mol / L; after the methylene blue solution and the catalyst are evenly mixed, they are stirred in the dark for 30 minutes and then irradiated under visible light. Samples are taken at regular intervals, centrifuged in a centrifuge, and the absorbance of the solution is tested using a UV-visible spectrophotometer.

[0110] Catalytic degradation of rhodamine solution experiment: The catalyst dosage is 0.1g per 100ml of rhodamine solution, and the concentration of rhodamine solution is 10 -5 mol / L. After the rhodamine solution and the catalyst were mixed evenly, they were stirred in the dark for 30 minutes and then irradiated under visible light. Samples were taken at regular intervals, centrifuged in a centrifuge, and the absorbance of the solution was tested using a UV-visible spectrophotometer.

[0111] In this embodiment, the effect of BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction on catalysis of methylene blue is as follows Figure 2 As the illumination time increases, the absorbance of the solution decreases significantly. When the visible light is illuminated for 5 hours, the degradation rate of methylene blue solution is 92%. Figure 3 When exposed to visible light for 8 hours, the degradation rate of methylene blue solution was 60%.

[0112] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, characterized in that: The method comprises the following preparation steps: 1) preparing a suspension containing bismuth and tungsten oxyhydroxide precipitates; 2) transferring the suspension prepared in step 1) into the inner tank of a reaction kettle, adjusting the volume of the suspension in the inner tank of the reaction kettle to 70-90% of the volume of the inner tank of the reaction kettle with deionized water, and stirring evenly to obtain a mixed solution; 3) adding bismuth ferrite single crystal nanosheets to the mixed solution prepared in step 2), stirring evenly to obtain a reaction material; 4) placing the reaction vessel liner containing the reaction materials in step 3) in the reaction vessel, sealing it, and performing hydrothermal treatment at 150-200° C. for 4.5-24 hours; 5) After the hydrothermal reaction is completed, the reactor is allowed to cool naturally to room temperature, and the reaction product is repeatedly washed with deionized water and anhydrous ethanol, filtered, and dried to obtain a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst; The bismuth tungstate of the BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst can be distributed at intervals on the bismuth ferrite single crystal nanosheets and present a sheet-like structure growth perpendicular to the bismuth ferrite.

2. The method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst according to claim 1, characterized in that: In the step 1), the preparation steps of the suspension containing bismuth and tungsten oxyhydroxide precipitates are: S1: prepare bismuth nitrate-dilute nitric acid solution; prepare sodium tungstate aqueous solution; S2: Mix the two solutions prepared in S1 and stir them evenly to obtain a mixed solution; S3: adding potassium hydroxide aqueous solution to the mixed solution prepared in S2, adjusting the solution pH to 6, and fully stirring at room temperature to obtain a suspension containing bismuth and tungsten hydroxide oxide precipitates.

3. The method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst according to claim 2, characterized in that: The specific steps of step S1 are: weighing bismuth nitrate and sodium tungstate in a molar ratio of 2:1, dissolving bismuth nitrate in 15% dilute nitric acid to obtain a bismuth nitrate-dilute nitric acid solution; and dissolving sodium tungstate in deionized water to obtain a sodium tungstate aqueous solution.

4. The method for preparing a BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst according to claim 3, characterized in that: The molar ratio of the sodium tungstate to the bismuth ferrite is 0.05-0.2:

1.

5. A BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst, characterized in that: The method is prepared by any one of claims 1 to 4.

6. An application of the BiFeO3 / Bi2WO6 two-dimensional single crystal heterojunction photocatalyst as claimed in claim 5, characterized in that: Used to catalyze the degradation of methylene blue and rhodamine under visible light.

Citation Information

Patent Citations

  • Preparation method of bismuth ferrite BiFeO3 monocrystal micrometer sheet

    CN102877130B

  • Preparation method of bismuth ferrite BiFeO3 monocrystal micrometer sheet

    CN102877130A

  • Bi2WO6-BiFeO3 compound photocatalyst and preparing method thereof

    CN105772018A

  • Bismuth ferrite / bismuth tungstate heterojunction photocatalytic material and preparation method thereof

    CN108435194A