A kind of MoS2 / layered silicate nanocomposite catalyst modified by additive and its preparation and application

MoS2 is modified with the nanocomposite of layered silicate by additives to form a vertical composite structure, which solves the problem of low exposure to catalytic active sites, and achieves efficient removal of a variety of heteroatoms and achieves the production of clean oil products that meet national standards.

CN116273067BActive Publication Date: 2024-11-26DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111520702.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-13
Publication Date
2024-11-26
Estimated Expiration
2041-12-13

AI Technical Summary

Technical Problem

The existing MoS2 catalysts have low exposure to catalytic active sites during the hydrorefining process, making it difficult to remove multiple heteroatoms in the distillate oil at one time, resulting in low production efficiency and quality of cleaning oil products.

Method used

MoS2 modified by additives is combined with layered silicate nanometers to form a vertical composite structure, increasing the exposure of catalytic active sites, and evenly dispersing the additive metal in the catalyst to form a variety of coordination structures to achieve a variety of heteroatoms. Efficient removal.

Benefits of technology

The hydrorefining of various fractions in crude oil and heavy oil has been achieved, and the efficient removal of heteroatoms such as metals, sulfur, nitrogen, and oxygen has been achieved. The product quality has reached national standards, especially in gasoline, diesel and heavy oil. The de-release rate reaches more than 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DEST_PATH_IMAGE001
    Figure DEST_PATH_IMAGE001
  • Figure DEST_PATH_IMAGE002
    Figure DEST_PATH_IMAGE002
  • Figure DEST_PATH_IMAGE003
    Figure DEST_PATH_IMAGE003
Patent Text Reader

Abstract

The invention relates to a dispersed distillate oil hydrofining catalyst development technology in the field of industrial catalysis technology, and is an additive-modified MoS2 / layered silicate nanocomposite catalyst and its preparation and application. The additive-modified MoS2 / layered silicate nanocomposite catalyst comprises additive-modified MoS2 and a layered silicate monolayer disc, and is structurally a vertical compound of additive-modified 1T-MoS2 nanosheets on the surface of the monolayered silicate disc. The additive-modified MoS2 / layered silicate nanocomposite catalyst obtained by the invention can be used for hydrofining of each distillate oil in heavy crude oil and / or heavy oil hydrogenation products to produce clean oil products. The additive-modified 1T-MoS2 nanosheet active components are vertically compounded on the surface of the layered silicate disc, and after the additive modification, more hydrofining active sites are created on the basal plane and edge of the 1T-MoS2, which increases the exposure of the catalytic hydrogenation active sites, and can realize the rapid hydrofining of distillate oil to produce clean oil products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to a method for preparing an auxiliary agent-modified MoS2 / layered silicate nanocomposite catalyst, belonging to a catalyst preparation technology in the technical field of industrial catalysis. Background technology:

[0002] Transition metal sulfide MoS2 has a typical layered structure, with weak van der Waals forces between layers, which are easy to peel off. Each molybdenum atom in the monoatomic layer is surrounded by six sulfur atoms, exposing many Mo-S facets, which can be used as catalytic active centers. (See Chianelli, RR Catal. Rev. 2006, 48 (1), 1-41) Due to the special layered structure, anisotropy, electronic properties and precious metal-like properties of MoS2, the current research on this material is mainly focused on catalytic hydrogenation, electrocatalysis, electrode materials, photocatalysis, friction lubrication, electronic probes, hydrogen storage materials and many other fields. MoS2 has become a hot material in the fields of chemistry, physics, and materials science at home and abroad.

[0003] MoS2 layers are connected by weak van der Waals forces to form a multilayer stacked structure, and the distance between adjacent S-Mo-S layers is 0.62nm. According to the different stacking methods, MoS2 has three polytypes: 2H, 3R and 1T. Among them, the 2H type is two triangular prism-coordinated S-Mo-S layers stacked to form a unit cell, and the stacking method of the layers is AB AB...; 3R is three triangular prism-coordinated S-Mo-S layers stacked to form a unit cell, and the order of layer stacking is ABC ABC..., and each unit cell in the 1T type contains one octahedral-coordinated S-Mo-S layer, and the stacking method of the layers is AA.... However, the two common crystal structures of molybdenum disulfide that can be chemically synthesized are: the stable 2H semiconductor state and the highly active metastable 1T phase MoS2 metallic state. The 1T phase structure of MoS2 has metallic properties due to its sulfur-rich characteristics and unique anisotropy. Therefore, compared with the 2H semiconductor state of MoS2, the 1T phase MoS2 has higher catalytic hydrogenation activity.

[0004] The heavy oil hydrogenation lightening products and the developed heavy oil crude oil distillates with different boiling points still contain a large amount of metals, sulfur, nitrogen, oxygen and other heteroatoms, and they still need to be hydrotreated to meet national standards before they can be directly used. Therefore, it is very important to develop efficient catalysts to further hydrotreate the distillates to produce high-quality clean oil products. Due to the increasing interest in the research of layered MoS2 materials, and because of their high hydrogenation activity and good anti-poisoning ability, they are widely used as catalysts in the oil refining industry, such as oil hydrogenation and quality improvement, including hydrogenation reactions, hydrodesulfurization, hydrodeoxygenation, hydrodenitrogenation and hydrodemetallization reactions. (See Prins, R. et al. Catal. Today 2006, 111 (1–2), 84-93) The catalytic hydrogenation activity of MoS2 materials is closely related to their structural characteristics. Since the catalytic hydrogenation active centers of MoS2 are mainly located on the edges, the surface energy is relatively high, which is 0.7 J / m 2 The surface is active, unstable, easy to agglomerate, and has few active centers exposed for catalytic hydrofining reactions. The active sites of catalytic hydrofining cannot achieve multiple reactions such as hydrodemetallization, desulfurization, denitrogenation, and deoxygenation at one time. It is urgent to develop effective catalysts to achieve distillate oil hydrofining to produce clean oil products at one time. Summary of the invention:

[0005] The present invention provides a MoS2 / layered silicate nanocomposite catalyst modified by an additive, and its preparation and application. The MoS2 with a metallic 1T structure modified by an additive has a hydrogenation activity with more types of coordination and a noble metal-like property, which overcomes the shortcomings of the above-mentioned prior art. The preparation of MoS2 with a 1T structure and rich active sites and the vertical compounding of MoS2 nanosheets on the surface of layered silicate are achieved through additive modification, which increases the exposure of the catalytic active sites of MoS2 and realizes the hydrogenation removal of various heteroatoms in various fractions in crude oil and / or heavy oil hydrogenation products at one time. The present invention can effectively solve the problem of low exposure of the catalyst active sites in the process of preparing clean oil products by liquid-phase hydrogenation refining of distillate oil, and remove heteroatoms such as metals, sulfur, nitrogen, and oxygen at the same time, and produce clean oil products that meet national use standards.

[0006] The technical solution of the present invention is achieved by the following measures:

[0007] The present invention provides a MoS2 / layered silicate nanocomposite catalyst modified by an additive, which comprises additive-modified MoS2 and a layered silicate monolayer disc, and is a vertical compound of additive-modified 1T-MoS2 nanosheets on the surface of the monolayered silicate disc. The additive elements in the additive-modified 1T-MoS2 nanosheets can be distributed on the basal plane and edge of the 1T-MoS2, the additive-modified 1T-MoS2 nanosheets are vertically compounded on the layered silicate surface, the farthest distance between the side edges of the additive-modified 1T-MoS2 nanosheets is 10 to 50 nm, the sheet thickness is 0.5 to 3.0 nm, the diameter of the monolayered silicate disc is 20 to 100 nm, and the disc thickness is 0.5 to 2.0 nm.

[0008] A method for preparing a MoS2 / layered silicate nanocomposite catalyst modified by an additive is obtained by the following steps:

[0009] (1) dispersing at least one of nano-sized natural clay, bentonite, synthetic Laponite and chemically synthesized layered silicate in water, and forming a colorless transparent sol under the action of at least one mechanical external force selected from the group consisting of high-speed shear emulsification, mechanical stirring, magnetic stirring and manual stirring;

[0010] (2) at least one of ammonium molybdate, sodium molybdate, molybdenum oxide, phosphomolybdic acid, and ammonium tetrathiomolybdate is used as a molybdenum source, at least one of soluble ammonium tetrathiomolybdate, sodium sulfide, potassium sulfide, ammonium sulfide, thiourea, carbon disulfide thioacetamide, cysteine, and glutathione is used as a sulfur source, at least one of nitrates, chlorides, sulfates, acetates, citrates, and oxalates of cobalt, nickel, and iron is used as a modified metal source, and at least one of a reducing sulfur source (one or more of cysteine, glutathione, thioacetamide, and thiourea), hydrazine hydrate, hydroxylamine hydrochloride, oxalic acid, and citric acid is dissolved in water as a reducing agent to form a MoS2 precursor solution; in the precursor solution, the molar ratio of the modified metal / Mo in the precursor is 1:20 to 1:2, the molar ratio of (auxiliary agent + Mo) / S is 1:4 to 1:6, and the molar ratio of Mo / reducing agent is 1:1 to 1:2.

[0011] (3) The silicate sol obtained in (1) and the additive-modified MoS2 precursor solution obtained in (2) are mixed under the action of at least one mechanical external force selected from the group consisting of high-speed shear emulsification, mechanical stirring, magnetic stirring, and manual stirring to form a uniform mixed sol; the mass ratio of silicate to additive-modified MoS2 in the mixed sol is 1 to 10, preferably 2 to 5.

[0012] (4) The mixed sol obtained in (3) can be further crystallized at 120-220° C. for 3-72 hours, preferably at 140-180° C. for 24-48 hours. The crystallization method can be a common crystallization method such as heating crystallization in a closed system oven, electric furnace, etc., microwave heating crystallization, open system oil bath heating crystallization, etc.; the product separation in the formed gel can be a product separation method such as polar solvent sedimentation separation, vacuum filtration separation and centrifugal separation, the product washing can be washed with deionized water and ethanol, and the product drying can be vacuum drying, freeze drying, CO2 supercritical drying, natural air drying, etc. to obtain an additive-modified MoS2 / layered silicate nanocomposite catalyst.

[0013] The MoS2 / layered silicate nanocomposite catalyst modified by the additive prepared by the present invention can be used for gasoline (components with a boiling point lower than 180°C), diesel (fractions with a boiling point of 180-350°C), distillate oil (fractions with a boiling point of 350-500°C) and heavy oil (components with a boiling point of 500-1000°C) in the hydrogenation products of crude oil and / or heavy oil for liquid-phase hydrogenation demetallization, desulfurization, denitrogenation and deoxygenation to prepare clean oil products, wherein the suspended bed liquid-phase hydrogenation reaction conditions are: the mass percentage of the catalyst is 0.1-1.0%; the reaction temperature is 300-400°C; and the reaction pressure is 6-10MPa.

[0014] The characterization analysis of the catalyst of the present invention is as follows: The mapping characterization results of the MoS2 / layered silicate nanocomposite catalyst modified by the additive of the present invention show that the additive in the MoS2 / layered silicate nanocomposite catalyst modified by the additive is uniformly dispersed on the basal plane and edge of the MoS2 layer (see Figure 1-3 ), can create active sites with various coordination structures, thus realizing the creation of MoS2 catalytic active sites. The results of Raman spectroscopy and electron paramagnetic resonance spectroscopy showed that the MoS2 sheets modified by the additive were 1T structured MoS2, which had precious metal-like properties and better hydrogenation activity. The STEM characterization results showed that the MoS2 sheets modified by the additive were 1T structured MoS2 sheets with vertical layered silicate surface composites, which effectively avoided the agglomeration and growth of MoS2 nanosheets.

[0015] Compared with the prior art, the present invention has the following advantages and effects:

[0016] (1) The present invention utilizes a layered silicate material in an aqueous solution to achieve high dispersion of the lamellae into a single charged disk by mechanical external force, wherein the lamellae have a diameter of 20 to 100 nm and are in a sol state, thereby fully interacting with the MoS2 nanosheets modified by the additive to achieve vertical recombination. In the process of static crystallization without mechanical external force, the layered silicate can form a gel state, thereby inhibiting the aggregation and growth of the MoS2 nanosheets modified by the additive, ensuring uniform dispersion and vertical recombination of 1T-MoS2, thereby achieving full exposure of the catalytic active sites.

[0017] (2) In the additive-modified MoS2 / layered silicate nanocomposite catalyst prepared by the present invention, the additive metal can be dispersed on the basal plane and edge position of the MoS2 nanosheet, and form a variety of coordination structures with Mo atoms and S atoms. The modified additive metal forms a variety of catalytic active sites with different coordination unsaturated structures on the edge position and basal plane of the metastable metallic 1T-MoS2, thereby achieving the removal of multiple heteroatoms in the distillate oil at one time.

[0018] (3) The additive-modified MoS2 / layered silicate nanocomposite catalyst prepared by the present invention is used for the hydrogenation products of crude oil and / or heavy oil, such as gasoline (components with a boiling point below 180°C), diesel (fractions with a boiling point of 180-350°C), distillate oil (fractions with a boiling point of 350-500°C) and heavy oil (components with a boiling point of 500-1000°C) to produce clean oil products by liquid phase hydrogenation demetallization, desulfurization, denitrogenation and deoxygenation of distillate oils, and the catalytic reaction results are shown in Table 1. The catalyst of the present invention is used for the hydrorefining of various distillate oils, and the metal removal rate in heavy oil can be as high as 95%, and the removal rate of nitrogen, oxygen and sulfur heteroatoms in distillate oil and diesel can be as high as 90%. The sulfur content in the gasoline hydrorefining product is only 8ppm, and the product quality meets the National Five Standard. Description of the drawings:

[0019] Figure 1 Mapping diagram of the Co-modified MoS2 / layered silicate sample obtained in Example 1.

[0020] Figure 2 Mapping diagram of the Ni-modified MoS2 / layered silicate sample obtained in Example 3.

[0021] Figure 3 Mapping diagram of the Fe-modified MoS2 / layered silicate sample obtained in Example 4.

[0022] Figure 4 Schematic diagram of the three polytypes of MoS2: 1T, 2H, and 3R. Specific implementation method:

[0023] In order to further illustrate the present invention, embodiments are given below, but they do not limit the scope of the present invention.

[0024] Embodiment 1:

[0025] Weigh 1.0g of Laponite (Bick Additives, USA, synthetic sodium magnesium silicate lithium salt, average particle size 60nm, single-layer disc size 25nm, single-layer disc thickness 0.92nm) and disperse it in 60ml of deionized water. Shear emulsify it at 13000r.mp for 10 minutes to form a colorless and transparent sol. Weigh 0.1104g of ammonium heptamolybdate, 0.0182g of cobalt nitrate hexahydrate, and 0.3781g of cysteine ​​and dissolve them in 60ml of water under stirring to form a red Co-modified MoS2 precursor solution. Under shear emulsification conditions, evenly mix the above Laponite sol and the Co-modified MoS2 precursor solution for 10 minutes to obtain a deep red sol. The resulting red sol is transferred to a stainless steel hydrothermal kettle with a polytetrafluoroethylene liner and crystallized at 160°C in an electric furnace for 24 hours. After cooling to room temperature, the solid was separated by suction filtration and washed three times with deionized water to obtain a black solid, which was freeze-dried for 12 hours to obtain a Co-modified MoS2 / Laponite nanocomposite catalyst.

[0026] The test results of nano-laser particle size analyzer show that the average particle size of Co-modified MoS2 / Laponite composite catalyst is 65nm, so Co-modified MoS2 / Laponite is a nano-composite catalyst. Mapping characterization results show that the Co element in the obtained Co-modified MoS2 / Laponite nano-composite catalyst is uniformly dispersed on the basal plane and edge of the MoS2 layer. The research results of Raman spectrometer and electron paramagnetic resonance spectrometer show that the Co-modified MoS2 layer in the Co-modified MoS2 / Laponite composite catalyst is 1T structure MoS2, which has the properties of precious metals. STEM electron microscope characterization results show that the Co-modified MoS2 layer is composited on the surface of vertical layered Laponite disks, and the farthest distance between the sides on the surface of the Co-modified MoS2 layer is 28nm, and the thickness is 1.8nm.

[0027] The catalyst prepared in this example is used for the hydrorefining reaction of heavy oil components with a boiling point of 500-1000° C. in Boskan oil. The suspended bed hydrogenation reaction conditions are: the mass percentage of the catalyst is 0.25% of the raw material; the reaction temperature is 350° C.; the hydrogen reaction pressure is 8 MPa. The metal removal rate after the hydrodemetallization reaction is as high as 95%, and the heteroatom removal rate after the hydrodesulfurization, denitrogenation and deoxygenation reactions is higher than 90%, which are much higher than the heteroatom removal rate of the comparative catalyst (see Table 1).

[0028] Embodiment 2:

[0029] Weigh 1.0g of lithium magnesium silicate (lithium magnesium silicate synthesized by hydrothermal method, with an average particle size of 180nm, a single-layer disc size of 80nm, and a single-layer disc thickness of 1.0nm measured by a nano-laser particle size analyzer) and disperse it in 60ml of deionized water. Shear emulsify it for 10 minutes at 13000 rmp to form a colorless and transparent sol. Weigh 1.1040g of ammonium heptamolybdate, 0.7434g of cobalt chloride hexahydrate, and 3.7812g of cysteine ​​and dissolve them in 60ml of water under stirring to form a red Co-modified MoS2 precursor solution. Under shear emulsification conditions, evenly mix the above-mentioned lithium magnesium silicate sol and the Co-modified MoS2 precursor solution for 10 minutes to obtain a deep red sol. The resulting red sol is transferred to a polytetrafluoroethylene liner and placed in a microwave synthesizer, and crystallized at 180°C in an oven for 6 hours. After cooling to room temperature, centrifugation was performed, and deionized water was washed three times to obtain a black solid, which was vacuum dried for 12 hours to obtain a Co-modified MoS2 / lithium magnesium silicate nanocomposite catalyst.

[0030] The test results of nano-laser particle size analyzer show that the average particle size of Co-modified MoS2 / lithium magnesium silicate composite catalyst is 98nm, so Co-modified MoS2 / lithium magnesium silicate is a nano-composite catalyst. Mapping characterization results show that the Co element in the obtained Co-modified MoS2 / lithium magnesium silicate nano-composite catalyst is uniformly dispersed on the basal plane and edge of the MoS2 layer. The research results of Raman spectrometer and electron paramagnetic resonance spectrometer show that the Co-modified MoS2 layer in the Co-modified MoS2 / lithium magnesium silicate composite catalyst is 1T structure MoS2, which has the properties of precious metals. The STEM electron microscope characterization results show that the Co-modified MoS2 layer is composited on the surface of the vertical layered lithium magnesium silicate disk, and the farthest distance between the side edges of the Co-modified MoS2 layer surface is 47nm, and the thickness is 1.4nm.

[0031] The catalyst prepared in this example is used for the hydrorefining reaction of heavy oil components with a boiling point of 500-1000° C. in Boskan crude oil. The suspended bed hydrogenation reaction conditions are: the mass percentage of the catalyst is 0.25% of the raw material; the reaction temperature is 350° C.; the hydrogen reaction pressure is 8 MPa. The metal removal rate after the hydrodemetallization reaction is as high as 93.4%, and the heteroatom removal rate after the hydrodesulfurization, denitrogenation and deoxygenation reactions is higher than 90%, which are much higher than the heteroatom removal rate of the comparative catalyst (see Table 1).

[0032] Embodiment 3:

[0033] Weigh 1.0g magnesium silicate (magnesium silicate synthesized by hydrothermal method, with an average particle size of 80nm, a single-layer disc size of 35nm, and a single-layer disc thickness of 0.95nm measured by a nano-laser particle size analyzer) and disperse it in 60ml deionized water, and mechanically stir for 1 hour to form a colorless and transparent sol. Weigh 0.8125g ammonium tetrathiomolybdate, 0.2728g nickel nitrate hexahydrate, and 0.5ml hydrazine hydrate and dissolve them in 60ml water under stirring to form a red Ni-modified MoS2 precursor solution. Under shear emulsification conditions, the above-mentioned magnesium silicate sol and the Ni-modified MoS2 precursor solution are uniformly mixed for 10 minutes to obtain a deep red sol. The resulting red sol is transferred to a polytetrafluoroethylene liner and placed in a microwave synthesizer, and crystallized at 180°C for 12 hours. After cooling to room temperature, it is filtered after sedimentation, washed with deionized water 3 times, and washed with ethanol 3 times to obtain a black solid, which is naturally dried for 24 hours to obtain a Ni-modified MoS2 / magnesium silicate nanocomposite catalyst.

[0034] The test results of nano-laser particle size analyzer show that the average particle size of Ni-modified MoS2 / magnesium silicate composite catalyst is 54nm, so Ni-modified MoS2 / magnesium silicate is a nano-composite catalyst. Mapping characterization results show that the Ni element in the obtained Ni-modified MoS2 / magnesium silicate nano-composite catalyst is uniformly dispersed on the basal plane and edge of the MoS2 layer. The research results of Raman spectrometer and electron paramagnetic resonance spectrometer show that the Ni-modified MoS2 layer in the Ni-modified MoS2 / magnesium silicate composite catalyst is 1T structure MoS2, which has the properties of precious metals. The STEM electron microscope characterization results show that the Ni-modified MoS2 layer is composited vertically on the surface of the magnesium silicate disk, the farthest distance between the side edges of the surface of the Ni-modified MoS2 layer is 25nm, and the thickness is 1.0nm.

[0035] The catalyst prepared in this example was used for the hydrorefining reaction of the distillate oil with a boiling point of 350-500° C. in Boskan crude oil. The suspended bed hydrogenation reaction conditions were: the mass percentage of the catalyst was 0.25% of the raw material; the reaction temperature was 350° C.; the hydrogen reaction pressure was 8 MPa. The heteroatom removal rate after the hydrodesulfurization, denitrogenation and deoxygenation reactions was higher than 90%, which was much higher than the heteroatom removal rate of the comparative catalyst (see Table 1).

[0036] Embodiment 4:

[0037] Weigh 1.0g magnesium silicate (magnesium silicate synthesized by hydrothermal method, with an average particle size of 80nm, a single-layer disc size of 35nm, and a single-layer disc thickness of 0.95nm measured by a nano-laser particle size analyzer) and disperse it in 30ml deionized water, and stir it magnetically for 1 hour to form a colorless and transparent sol. Weigh 1.6258g ammonium tetrathiomolybdate, 0.5050g ferric nitrate nonahydrate, and 1ml hydrazine hydrate and dissolve them in 90ml water under stirring to form a red Fe-modified MoS2 precursor solution. Under magnetic stirring conditions, the above-mentioned magnesium silicate sol and the Fe-modified MoS2 precursor solution are uniformly mixed for 1 hour to obtain a dark red sol. The resulting red sol is transferred to a hydrothermal kettle with a polytetrafluoroethylene liner and crystallized at 200°C in an oven for 16 hours. After cooling to room temperature, centrifugation is performed, and deionized water is washed 3 times to obtain a black solid, which is vacuum dried for 24 hours to obtain a Fe-modified MoS2 / magnesium silicate nanocomposite catalyst.

[0038] The test results of nano-laser particle size analyzer show that the average particle size of Fe-modified MoS2 / magnesium silicate composite catalyst is 78nm, so Fe-modified MoS2 / magnesium silicate is a nano-composite catalyst. Mapping characterization results show that the Fe element in the obtained Fe-modified MoS2 / magnesium silicate nano-composite catalyst is uniformly dispersed on the basal plane and edge of the MoS2 layer. The research results of Raman spectrometer and electron paramagnetic resonance spectrometer show that the Fe-modified MoS2 layer in the Fe-modified MoS2 / magnesium silicate composite catalyst is 1T structure MoS2, which has the properties of precious metals. The STEM electron microscope characterization results show that the Fe-modified MoS2 layer is composited vertically on the surface of the magnesium silicate disk, the farthest distance between the side edges of the Fe-modified MoS2 layer surface is 39nm, and the thickness is 2.3nm.

[0039] The catalyst prepared in this embodiment is used for the hydrofining reaction of the diesel fraction with a boiling point of 180-350°C in Boskan crude oil. The suspended bed hydrogenation reaction conditions are: the mass percentage of the catalyst is 0.25% of the original; the reaction temperature is 350°C; the hydrogen reaction pressure is 8MPa, and the heteroatom removal rate after hydrodesulfurization, denitrogenation and deoxygenation is higher than 90%, which is much higher than the heteroatom removal rate of the comparative catalyst. In particular, the sulfur content can be reduced to 10ppm after the hydrodesulfurization reaction, reaching the National Five Standard (see Table 1).

[0040] Embodiment 5:

[0041] Weigh 1.0g of sodium bentonite (Shanghai Aladdin Biochemical Technology Co., Ltd., natural clay, average particle size 90nm, single-layer disc size 50nm, single-layer disc thickness 1.0nm) and disperse it in 30ml of deionized water, and stir magnetically for 1 hour to form a colorless and transparent sol. Weigh 1.2870g of sodium molybdate, 0.6221g of nickel acetate tetrahydrate, 2.3750g of thiourea, and 0.8688g of hydroxylamine hydrochloride are dissolved in 90ml of water under stirring to form a red Ni-modified MoS2 precursor solution. Under magnetic stirring conditions, the above-mentioned sodium bentonite sol and the Ni-modified MoS2 precursor solution are uniformly mixed for 1 hour to obtain a dark red sol. The resulting red sol is transferred to a hydrothermal kettle with a polytetrafluoroethylene liner and crystallized at 200°C in an oven for 16 hours. After cooling to room temperature, the solid was directly filtered and washed with deionized water three times to obtain a black solid, which was then vacuum dried for 24 hours to obtain a Ni-modified MoS2 / sodium-based bentonite nanocomposite catalyst.

[0042] The test results of nano-laser particle size analyzer show that the average particle size of Ni-modified MoS2 / sodium-based swellable composite catalyst is 88nm, so Ni-modified MoS2 / sodium-based swellable is a nano-composite catalyst. Mapping characterization results show that the Ni element in the obtained Ni-modified MoS2 / sodium-based swellable nano-composite catalyst is uniformly dispersed on the basal plane and edge of the MoS2 layer. The research results of Raman spectrometer and electron paramagnetic resonance spectrometer show that the Ni-modified MoS2 layer in the Ni-modified MoS2 / sodium-based swellable composite catalyst is 1T structure MoS2, which has the properties of precious metals. The STEM electron microscope characterization results show that the Ni-modified MoS2 layer is composited vertically on the surface of the sodium-based swellable disk, and the farthest distance from the side of the surface of the Ni-modified MoS2 layer is 45nm, and the thickness is 2.1nm.

[0043] The catalyst prepared in this embodiment is used for the hydrofining reaction of gasoline fraction with a boiling point below 180°C in Boskan crude oil. The suspended bed hydrogenation reaction conditions are: the mass percentage of the catalyst is 0.25% of the raw material; the reaction temperature is 350°C; the hydrogen reaction pressure is 8MPa, and the removal rate of heteroatoms after hydrodesulfurization, denitrogenation and deoxygenation is higher than 90%, which is much higher than the heteroatom removal rate of the comparative catalyst. The sulfur content after hydrodesulfurization reaction can be reduced to 10ppm, reaching the National Five Standard (see Table 1).

[0044] Embodiment 6:

[0045] Weigh 1.0g sodium bentonite (Shanghai Aladdin Biochemical Technology Co., Ltd., natural clay, average particle size 90nm, monolayer disc size 50nm, monolayer disc thickness 1.0nm) and disperse in 30m deionized water, 13000r.mp shear emulsification for 10 minutes to form a colorless transparent sol. Weigh 0.9600g phosphomolybdic acid, 0.3324g ferric citrate monohydrate, 2.8125g thioacetamide, 1.2001g citric acid and stir and dissolve in 90ml water to form a red Fe-modified MoS2 precursor solution. Under shear emulsification conditions, the above sodium bentonite sol and Fe-modified MoS2 precursor solution were uniformly mixed for 10 minutes to obtain a dark red sol. The resulting red sol was transferred to a round-bottomed flask with a reflux device and crystallized at 120°C in an oil bath for 60 hours. After cooling to room temperature, the solid was filtered after sedimentation and washed with deionized water three times to obtain a black solid. After freeze-drying for 6 hours, the Fe-modified MoS2 / sodium-based bentonite nanocomposite catalyst was obtained.

[0046] The test results of nano-laser particle size analyzer show that the average particle size of Fe-modified MoS2 / sodium-based swellable composite catalyst is 76nm, so Fe-modified MoS2 / sodium-based swellable is a nano-composite catalyst. Mapping characterization results show that the Fe element in the obtained Fe-modified MoS2 / sodium-based swellable nano-composite catalyst is uniformly dispersed on the basal plane and edge of the MoS2 layer. The research results of Raman spectrometer and electron paramagnetic resonance spectrometer show that the Fe-modified MoS2 layer in the Fe-modified MoS2 / sodium-based swellable composite catalyst is 1T structure MoS2, which has the properties of precious metals. The STEM electron microscope characterization results show that the Fe-modified MoS2 layer is composited vertically on the surface of the sodium-based swellable disk, and the farthest distance from the side of the surface of the Fe-modified MoS2 layer is 34nm, and the thickness is 0.8nm.

[0047] The catalyst prepared in this embodiment is used for the hydrofining reaction of gasoline fraction with a boiling point below 180°C in Boskan crude oil. The suspended bed hydrogenation reaction conditions are: the mass percentage of the catalyst is 0.25% of the raw material; the reaction temperature is 350°C; the hydrogen reaction pressure is 8MPa, and the removal rate of heteroatoms after hydrodesulfurization, denitrogenation and deoxygenation is higher than 90%, which is much higher than the heteroatom removal rate of the comparative catalyst. The sulfur content after hydrodesulfurization reaction can be reduced to 10ppm, reaching the National Five Standard (see Table 1).

[0048] Comparative Example 1:

[0049] Weigh 0.1104g of ammonium heptamolybdate and 0.3781g of cysteine ​​and dissolve them in 60ml of water under stirring to form a red MoS2 precursor solution. The resulting red solution was transferred to a stainless steel hydrothermal reactor with a polytetrafluoroethylene liner and crystallized at 160°C for 24 hours. After cooling to room temperature, the solid was separated by suction and washed with deionized water three times to obtain a black solid. After freeze drying for 12 hours, a pure MoS2 catalyst was obtained.

[0050] Nano-laser particle size test results show that the average particle size of pure MoS2 catalyst is 270nm. SEM characterization results show that the pure MoS2 catalyst obtained in the comparative example is an aggregate of MoS2 nanosheets, with less exposure of catalytic hydrogenation active sites. Raman spectrometer and electron paramagnetic resonance spectrometer research results show that the MoS2 catalyst is a 2H structure MoS2 with semiconductor properties.

[0051] Comparative Example 2:

[0052] Weigh 0.1104g of ammonium heptamolybdate, 0.0182g of cobalt nitrate hexahydrate, and 0.3781g of cysteine ​​and dissolve them in 60ml of water under stirring to form a red Co-modified MoS2 precursor solution. The resulting red solution was transferred to a stainless steel hydrothermal kettle with a polytetrafluoroethylene liner and crystallized at 160°C in an electric furnace for 24 hours. After cooling to room temperature, the solid was separated by suction and washed with deionized water three times to obtain a black solid, which was freeze-dried for 12 hours to obtain a Co-modified MoS2 catalyst.

[0053] Nano-laser particle size test results show that the average particle size of the Co-modified MoS2 catalyst is 235nm. SEM characterization results show that the Co-modified MoS2 catalyst obtained in the comparative example is an aggregate of MoS2 nanosheets, with less exposure of catalytic hydrogenation active sites. Raman spectrometer and electron paramagnetic resonance spectrometer research results show that the MoS2 catalyst is a 2H structure MoS2 with semiconductor properties.

[0054] Comparative Example 3:

[0055] Weigh 1.0g Laponite (Bick Additives Co., Ltd., USA, artificially synthesized sodium magnesium silicate lithium salt, average particle size 60nm, single-layer disc size 25nm, single-layer disc thickness 0.92nm) and disperse it in 60ml deionized water. Shear emulsify it for 10 minutes at 13000r.mp to form a colorless and transparent sol. Weigh 0.1104g ammonium heptamolybdate and 0.2556g cysteine ​​and dissolve them in 60ml water under stirring to form a red MoS2 precursor solution. Under 13000r.mp shear emulsification conditions, the above Laponite sol and MoS2 precursor solution are uniformly mixed for 10 minutes to obtain a dark red sol. The obtained red sol is transferred to a stainless steel hydrothermal kettle with a polytetrafluoroethylene lining and crystallized at 160°C in an electric furnace for 24 hours. After cooling to room temperature, it is separated by suction filtration and washed with deionized water 3 times to obtain a black solid. After freeze-drying for 12 hours, a MoS2 / sodium magnesium silicate lithium composite catalyst is obtained.

[0056] The test results of the nano-laser particle size analyzer show that the average particle size of the MoS2 / sodium magnesium silicate lithium composite catalyst obtained in this embodiment is 30nm, so MoS2 / sodium magnesium silicate lithium is a nano-composite catalyst. The SEM characterization results of the MoS2 / sodium magnesium silicate lithium nano-composite catalyst show that the MoS2 component in the catalyst is a single nano-sheet of island-like composite on the surface of a single layered sodium magnesium silicate disk with a size of 20-30nm. The research results of Raman spectrometer and electron paramagnetic resonance spectrometer show that the MoS2 catalyst in MoS2 / sodium magnesium silicate lithium nano-composite catalyst is a 2H structure MoS2 with semiconductor properties. The HRTEM characterization results show that the number of stacked layers of a single MoS2 nano-sheet is 1, the sheet thickness is about 1.0nm, and the length of the two farthest points on the side of the sheet surface is 3-5nm.

[0057] The comparative catalysts prepared in Comparative Examples 1-3 were used for the hydrorefining reaction of heavy oil components with a boiling point of 500-1000°C in Boskan oil. The suspended bed hydrogenation reaction conditions were: the mass percentage of the catalyst was 0.25% of the raw material; the reaction temperature was 350°C; the hydrogen reaction pressure was 8MPa, and the removal rates of heteroatoms after the hydrodemetallization, desulfurization, denitrogenation and deoxygenation reactions are shown in Table 1.

[0058] Table 1 Distillate oil hydrorefining activities of the MoS2 / layered silicate nanocomposite catalyst modified by the additive prepared in the present invention and the control sample catalyst.

[0059]

[0060] Table 2. Heteroatom contents of various fractions in Boskan crude oil.

[0061]

Claims

1. A MoS2 / layered silicate nanocomposite catalyst modified by an additive, characterized in that: The additive-modified MoS2 / layered silicate nanocomposite catalyst comprises additive-modified MoS2 and layered silicate monolayer discs, and is a vertical composite of additive-modified 1T-MoS2 nanosheets on the surface of the monolayer silicate disc. One or more of cobalt, nickel and iron are used as auxiliary agents; the maximum distance between the side edges of the 1T-MoS2 nanosheets modified by the auxiliary agents is 10-50 nm, and the thickness of the sheet is 0.5-3.0 nm. The molar ratio of the additive metal / Mo in the additive-modified MoS2 / layered silicate nanocomposite catalyst is 1:20-1:2, and the mass ratio of the layered silicate to the additive-modified MoS2 in the composite catalyst is 1-10; the additive elements in the additive-modified 1T-MoS2 nanosheets can be distributed on the basal plane and edge of the 1T-MoS2; the diameter of the monolayer silicate disk is 20-100 nm, and the disk thickness is 0.5-2.0 nm; The preparation method of the MoS2 / layered silicate nanocomposite catalyst modified by an auxiliary agent comprises the following steps: (1) Dispersing layered silicate in water to form a colorless and transparent sol under the action of mechanical external force; (2) dissolving a molybdenum source, a sulfur source, a metal source, and a reducing agent in water to form an additive-modified MoS2 precursor solution; the metal source is one or a mixture of two or more of nitrates, chlorides, sulfates, acetates, citrates, and oxalates of cobalt, nickel, and iron; (3) mixing the silicate sol obtained in (1) and the additive-modified MoS2 precursor solution obtained in (2) under the action of a mechanical external force to form a uniform mixed sol; (4) subjecting the mixed sol obtained in (3) to crystallization treatment, separating the product in the formed gel, and fully drying to obtain an additive-modified MoS2 / layered silicate nanocomposite catalyst; The layered silicate used is one or a mixture of two or more of natural clay and chemically synthesized layered silicate with a particle size of 10 to 200 nm; The sulfur source used is one or a mixture of two or more of soluble ammonium tetrathiomolybdate, sodium sulfide, potassium sulfide, ammonium sulfide, thiourea, carbon disulfide, thioacetamide, cysteine, and glutathione; the reducing agent used is one or a mixture of two or more of a reducing sulfur source, hydrazine hydrate, hydroxylamine hydrochloride, oxalic acid, and citric acid; the reducing sulfur source is one or two or more of cysteine, glutathione, thioacetamide, and thiourea.

2. The MoS2 / layered silicate nanocomposite catalyst modified by an auxiliary agent according to claim 1, characterized in that: The mass ratio of layered silicate to MoS2 modified by auxiliary agent in the composite catalyst is 2-5; the layered silicate used is one or more of magnesium silicate, lithium magnesium silicate and sodium magnesium silicate lithium.

3. The MoS2 / layered silicate nanocomposite catalyst modified by an auxiliary agent according to claim 1, characterized in that: The molybdenum source used is one of ammonium molybdate, sodium molybdate, molybdenum oxide, phosphomolybdic acid, and ammonium tetrathiomolybdate, or a mixture of two or more thereof.

4. The MoS2 / layered silicate nanocomposite catalyst modified by an auxiliary agent according to claim 1, characterized in that: When a reducing sulfur source is used in step (2), it serves as both a sulfur source and a reducing agent; the molar ratio of (auxiliary agent + Mo) / S is 1:4-1:6, and the molar ratio of Mo / reducing agent is 1:1-1:

2.

5. The additive-modified MoS2 / layered silicate nanocomposite catalyst according to claim 1, characterized in that: The mass concentration of the layered silicate in the mixed sol of step (3) is in the range of 0.8 to 30 mg / ml; the crystallization temperature of the mixed sol of step 4 is in the range of 120 to 220°C, the crystallization time is in the range of 3 to 72 hours, and the crystallization time is in the range of 24 to 48 hours.

6. The additive-modified MoS2 / layered silicate nanocomposite catalyst according to claim 1, characterized in that: The mechanical external force used to form the sol of the layered silicate includes one or more of high-speed shear emulsification, mechanical stirring, magnetic stirring, and manual stirring.

7. The additive-modified MoS2 / layered silicate nanocomposite catalyst according to claim 1, characterized in that: The crystallization time in step (4) is 140-180°C.

8. A MoS2 / layered silicate nanocomposite catalyst modified by an auxiliary agent according to any one of claims 1 to 7 for use in crude oil and / or heavy oil hydrogenation products, for preparing clean oil products from the fractions having a boiling point lower than 180°C in gasoline, the fraction having a boiling point of 180-350°C in diesel, the fraction having a boiling point of 350-500°C in distillate oil, and the fraction having a boiling point greater than 500-1000°C in heavy oil.

9. The use of the additive-modified MoS2 / layered silicate nanocomposite catalyst according to claim 8, characterized in that: The additive-modified MoS2 / layered silicate nanocomposite catalyst is used for liquid phase hydrogenation demetallization, desulfurization, denitrogenation and deoxygenation of the components with boiling point below 180°C in gasoline of crude oil and / or heavy oil hydrogenation products, the fraction with boiling point between 180 and 350°C in diesel, the fraction with boiling point between 350 and 500°C in distillate oil and the fraction with boiling point between 500 and 1000°C in heavy oil to produce clean oil products. The suspended bed hydrogenation reaction conditions are as follows: the mass percentage of the catalyst is 0.1 to 1.0%; the reaction temperature is 300 to 400°C; and the hydrogen reaction pressure is 6 to 10MPa.

Citation Information

Patent Citations

  • Preparation of bulk metallic group viii / group vib metal catalysts

    CN101909747A

  • Methods for hydrodesulfurization, hydronitrogenation, hydrorefining, or amine production.

    CN102292418A

  • Supported MoS2 / LDHS hydrodesulfurization catalyst and application

    CN106268872A

  • Supported hydrogenation catalyst as well as preparation method and application thereof

    CN111715232A

  • Hydrofining catalyst, preparation method thereof and application of hydrofining catalyst in oil refining and aromatic ring saturation regulation

    CN113680347A