Solid high entropy catalyst and method for preparing the same and applying the same to prepare furan acrolein

Through the preparation of solid high-entropy catalysts and catalytic tandem reaction technology, the problem of high cost of precious metal catalysts is solved, and the efficient oxidation-condensation of furfural and fatty alcohols is achieved, with the advantages of high selectivity and strong economicality.

CN116273181BActive Publication Date: 2024-11-08TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211546386.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2024-11-08
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

Existing precious metal catalysts are costly to use in the oxidation-condensation reaction between furfural and fatty alcohols, limiting industrial applications, and lacking catalysts with high efficiency, recyclability and economicality.

Method used

The solid high entropy catalyst is prepared by components such as acetylacetone metal complex, anhydrous glucose and dodecyl trimethylammonium chloride. Combined with ultrasonic and drying treatment, a highly active catalyst is formed, and furfural is realized through catalytic tandem reaction technology. Selective oxidation-condensation with fatty alcohols, using oxygen as an oxidant.

Benefits of technology

It achieves the efficient and highly selective conversion of furfural, the raw materials are cheap and easy to obtain, the reaction conditions are mild, and the catalyst is easy to recover, which has the advantages of strong economical and sustainable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116273181B_ABST
    Figure CN116273181B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of chemical industry, and more particularly to a solid high entropy catalyst and its preparation and application in the preparation of furan acrolein. The preparation process of the solid high entropy catalyst is to use 0-1mol of acetylacetone metal complex, 0-1kg of anhydrous glucose, 0-1kg of dodecyl trimethyl ammonium chloride, i.e., 0-1kg of DTAC, and 0-50L of oleylamine solution, fully stir for 20min until it is dissolved, then ultrasonicate for 2h, and keep the completely dissolved solution at a temperature of 220°C for 5h to obtain a high entropy catalyst solution; add cyclohexane and ethanol mixed solution to the high entropy catalyst solution, centrifuge and wash 3 times, dry overnight in a 60°C vacuum drying oven, and grind to obtain a high entropy catalyst after drying. The present invention realizes efficient and highly selective conversion of furfural by catalytic cascade reaction technology, and the raw materials used are cheap and easy to obtain, the reaction conditions are mild, and the catalyst is easy to recover; compared with precious metal catalysts, it has the advantages of good economy, simple synthesis method, and strong sustainability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical industry, and in particular to a solid high entropy catalyst and a method for preparing the catalyst and applying the catalyst to prepare furan acrolein. Background Art

[0002] Furfural, as a biomass platform compound, has a special molecular structure and can undergo various types of chemical reactions to prepare a series of biomass derivatives. Its downstream products cover multiple industries such as medicine, coatings, and resins.

[0003] Currently, the oxidation-condensation reaction of furfural and fatty aldehydes is also an effective way to extend the carbon chain to produce longer hydrocarbon chains and high-value liquid fuels.

[0004] In addition, in previous studies, precious metals were used as catalysts, but their high cost limits their industrial applications.

[0005] Therefore, we designed and developed a new high-activity catalyst for efficient utilization of furfural. The catalyst has the advantages of safety, high efficiency, high conversion rate, high selectivity, recyclability, and green economy. Summary of the invention

[0006] The main purpose of the present invention is to solve the above problems and provide a method for preparing furan acrolein by promoting the selective oxidation-condensation of biomass-based furfural and fatty alcohols with a solid high entropy catalyst. The solid high entropy catalyst can be used to cause a catalytic series reaction between furfural and fatty alcohols. The reaction equation is as follows: Figure 1 .

[0007] In order to achieve the above object, the present invention adopts the following technical scheme:

[0008] A preparation method of a solid high-entropy catalyst comprises the following steps: using 0-1 mol of acetylacetone metal complex, 0-1 kg of anhydrous glucose, 0-1 kg of dodecyltrimethylammonium chloride (DTAC), and 0-50 L of oleylamine solution, stirring them fully for 20 minutes to dissolve them, ultrasonicating them for 2 hours, and keeping the completely dissolved solution at a temperature of 220°C for 5 hours to obtain a high-entropy catalyst solution; adding a mixed solution of cyclohexane and ethanol to the high-entropy catalyst solution, centrifugally washing it for 3 times, drying it in a vacuum drying oven at 60°C overnight, and grinding it after drying to obtain the high-entropy catalyst.

[0009] In the preparation method of the solid high-entropy catalyst, the acetylacetonate metal complex used is five or more of acetylacetonate iron, acetylacetonate manganese, acetylacetonate cobalt, acetylacetonate nickel, acetylacetonate platinum or acetylacetonate aluminum, wherein the above acetylacetonate metal complexes can be replaced by acetylacetonate complexes of metal copper, chromium, vanadium, lanthanum or cerium.

[0010] The solid high entropy catalyst prepared by the preparation method, the preparation process of the solid high entropy catalyst is:

[0011] Use 0-1 mol of acetylacetonate metal complex, 0-1 kg of anhydrous glucose, 0-1 kg of dodecyltrimethylammonium chloride (DTAC), and 0-50 L of oleylamine solution; stir thoroughly for 20 minutes to dissolve, then ultrasonicate for 2 hours, keep the completely dissolved solution at 220°C for 5 hours to obtain a high entropy catalyst solution, add cyclohexane and ethanol mixed solution to the high entropy catalyst solution, centrifuge and wash 3 times, dry in a 60°C vacuum drying oven overnight, dry and grind to obtain a high entropy catalyst; the acetylacetonate metal complex used is five or more of acetylacetonate iron, acetylacetonate manganese, acetylacetonate cobalt, acetylacetonate nickel, acetylacetonate platinum or acetylacetonate aluminum, wherein the above acetylacetonate metal complexes can be replaced by acetylacetonate complexes of metal copper, chromium, vanadium, lanthanum, and cerium.

[0012] The application method of the solid high entropy catalyst is applied to the reaction of biomass-based furfural and fatty alcohol selective oxidation-condensation to prepare furan acrolein, and the steps are: biomass-based furfural is used as a reaction substrate, alcohol is used as a solvent, a solid high entropy catalyst is added, an alkali auxiliary is added, heating and stirring are performed, and furfural and fatty alcohol undergo a catalytic series reaction, and the method is carried out using oxygen as an oxidant.

[0013] The fatty alcohol is one or more of ethanol, propanol, isopropanol, butanol, isobutanol, n-pentanol, n-hexanol, n-heptanol, n-octanol or isooctyl alcohol.

[0014] The alkali auxiliary agent is Li 2 CO 3 、Na 2 CO 3 , K 2 CO 3 , Cs 2 CO 3 , KHCO 3 、NaHCO 3 , LiOH, NaOH, KOH, SrOH, Ca(OH) 2 , CaO, sodium formate, sodium acetate, sodium propionate, sodium methoxide or sodium ethoxide.

[0015] The heating reaction temperature is 0-240°C, the reaction time is 0-60h, and the stirring rate is 0-9000r / min.

[0016] The mass percentage of the catalyst and the reaction substrate furfural is 0.0001-50%.

[0017] The reaction oxidant is one of oxygen, air, oxygen mixed gas, hydrogen peroxide or tert-butyl hydroperoxide.

[0018] The invention realizes the efficient and highly selective conversion of furfural by catalytic cascade reaction technology. The raw materials used are cheap and easily available, the reaction conditions are mild, and the catalyst is easy to recover. Compared with precious metal catalysts, the invention has the advantages of good economy, simple synthesis method, strong sustainability, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a chemical reaction formula for preparing furan acrolein by selective oxidation-condensation of biomass-based furfural and fatty alcohols promoted by solid high entropy catalyst. DETAILED DESCRIPTION

[0020] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer and more understandable, the present invention is further described in detail with examples below.

[0021] The specific operation mode of the present invention is as follows:

[0022] Weigh a certain amount of biomass-based furfural as a reaction substrate, use alcohol as a solvent, add a solid high-entropy catalyst, add an appropriate amount of alkali additive, add a magnet, remove the air in the system, fill with a certain pressure of oxygen, heat and stir, and the furfural and fatty alcohol react in a catalytic series reaction. After the reaction is completed, the high-entropy catalyst is separated from the solution through a syringe and a filter membrane, and the product is analyzed by gas chromatography.

[0023] Embodiment 1:

[0024] Preparation method of solid high entropy catalyst and its application in catalytic series reaction of furfural and ethanol:

[0025] 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) were added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) was added. After fully stirring for 20min to dissolve, the mixture was ultrasonicated for 2h. The completely dissolved solution was kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst was washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst was obtained by grinding. Take 0.025g of the above catalyst, 0.025g of Cs 2 CO 3 , 0.1 g furfural was added to a polytetrafluoroethylene autoclave, and then 10 mL ethanol solvent was added, and 0.3 MPaO 2, and heated to 130°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 73.62% and the yield of 3-(2-furanyl)acrolein was 71.51%.

[0026] Embodiment 2:

[0027] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-propanol:

[0028] 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) were added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) was added. After fully stirring for 20min to dissolve, the mixture was ultrasonicated for 2h. The completely dissolved solution was kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst was washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst was obtained by grinding. Take 0.025g of the above catalyst, 0.025g of Cs 2 CO 3 , 0.1 g furfural was added to a polytetrafluoroethylene autoclave, and then 10 mL of n-propanol solvent was added, and 0.3 MPaO 2 , and heated to 130°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 81.92%, and the yield of 3-(2-furanyl)-2-methyl-2-propenal was 80.98%.

[0029] Embodiment 3:

[0030] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-propanol:

[0031] 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) were added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) was added. After being fully stirred for 20min to dissolve, it was ultrasonicated for 2h. The completely dissolved solution was kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst was washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst was obtained by grinding. 0.025g of the above catalyst, 0.025g of LiOH, and 0.1g of furfural were added to a polytetrafluoroethylene high-pressure reactor, and 10mL of n-propanol solvent was added. 0.3MPaO 2 , and heated to 80°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 93.97% and the yield of 3-(2-furanyl)-2-methyl-2-propenal was 92.11%.

[0032] Embodiment 4:

[0033] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-butanol:

[0034] 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) were added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) was added. After being fully stirred for 20min to dissolve, it was ultrasonicated for 2h. The completely dissolved solution was kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst was washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst was obtained by grinding. 0.025g of the above catalyst, 0.025g of LiOH, and 0.1g of furfural were added to a polytetrafluoroethylene high-pressure reactor, and 10mL of n-butanol solvent was added. 0.3MPaO 2 , and heated to 80°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 99.77% and the yield of 3-(2-furanyl)-2-ethyl-2-propenal was 97.55%.

[0035] Embodiment 5:

[0036] Preparation method of solid high entropy catalyst and its application in catalytic series reaction of furfural and n-pentanol:

[0037] 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) were added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) was added. After being fully stirred for 20min to dissolve, it was ultrasonicated for 2h. The completely dissolved solution was kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst was washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, dried in a vacuum drying oven at 60℃ overnight, and ground after drying to obtain a high entropy catalyst. 0.025g of the above catalyst, 0.025g of LiOH, and 0.1g of furfural were added to a polytetrafluoroethylene high-pressure reactor, and 10mL of n-pentanol solvent was added. 0.3MPaO 2 , and heated to 80°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 99% and the yield of 3-(2-furanyl)-2-propyl-2-propenal was 88.14%.

[0038] Embodiment 6:

[0039] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-hexanol: 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) are added to 30mL of oleylamine, 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) is added, and the mixture is stirred for 20min to dissolve, and then ultrasonicated for 2h. The completely dissolved solution is kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst is washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst is obtained by grinding. 0.025g of the above catalyst, 0.025g of LiOH, and 0.1g of furfural are added to a polytetrafluoroethylene high-pressure reactor, and 10mL of n-hexanol solvent is added, 0.3MPaO2 is charged, and the mixture is stirred and heated to 80℃ for 2h. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 95%, and the yield of 3-(2-furanyl)-2-propyl-2-propenal was 87.17%.

[0040] Embodiment 7:

[0041] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-heptanol: 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) are added to 30mL of oleylamine, 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) is added, and the mixture is stirred for 20min to dissolve, and then ultrasonicated for 2h. The completely dissolved solution is kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst is washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst is obtained by grinding. 0.025g of the above catalyst, 0.025g of LiOH, and 0.1g of furfural are added to a polytetrafluoroethylene high-pressure reactor, and 10mL of n-heptanol solvent is added, 0.3MPaO2 is charged, and the mixture is stirred and heated to 80℃ for 2h. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 94.5%, and the yield of 3-(2-furanyl)-2-propyl-2-propenal was 86.37%.

[0042] Embodiment 8:

[0043] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-octanol: 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) are added to 30mL of oleylamine, 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) is added, and the mixture is stirred for 20min until dissolved, and then ultrasonicated for 2h. The completely dissolved solution is kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst is washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. The high entropy catalyst is obtained by grinding after drying. 0.025g of the above catalyst, 0.025g of LiOH, and 0.1g of furfural are added to a polytetrafluoroethylene high-pressure reactor, and 10mL of n-octanol solvent is added, 0.3MPaO2 is charged, and the mixture is stirred and heated to 80℃ for 2h. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 94.3%, and the yield of 3-(2-furanyl)-2-propyl-2-propenal was 85.55%.

[0044] Embodiment 9:

[0045] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-nonanol: 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) are added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) is added, and stirred for 20min to dissolve, and then ultrasonicated for 2h, and the completely dissolved solution is kept at 220℃ for 5h to obtain a high entropy catalyst, and the high entropy catalyst is washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight, and then ground to obtain a high entropy catalyst. Take 0.025g of the above catalyst, 0.025g of LiOH, and 0.1g of furfural and add them to a polytetrafluoroethylene high-pressure reactor, and then add 10mL of n-nonanol solvent, and fill with 0.3MPaO 2 , and heated to 80°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 92.3%, and the yield of 3-(2-furanyl)-2-propyl-2-propenal was 83.35%.

[0046] Embodiment 10:

[0047] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-decanol: 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) are added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) is added, and stirred for 20min to dissolve, and then ultrasonicated for 2h, and the completely dissolved solution is kept at 220℃ for 5h to obtain a high entropy catalyst, and the high entropy catalyst is washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight, and then ground to obtain a high entropy catalyst. Take 0.025g of the above catalyst, 0.025g of LiOH, and 0.1g of furfural and add them to a polytetrafluoroethylene high-pressure reactor, and then add 10mL of n-decanol solvent, and fill with 0.3MPaO 2 , and heated to 80°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 90.13%, and the yield of 3-(2-furanyl)-2-propyl-2-propenal was 81.34%.

[0048] Embodiment 11:

[0049] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-propanol:

[0050] 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) were added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) was added. After being fully stirred for 20min to dissolve, it was ultrasonicated for 2h. The completely dissolved solution was kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst was washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst was obtained by grinding. Take 0.025g of the above catalyst, 0.025gK 2 CO 3 , 0.1 g furfural was added to a polytetrafluoroethylene autoclave, and then 10 mL of n-propanol solvent was added, and 0.3 MPaO 2 , and heated to 130°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 80.92% and the yield of 3-(2-furanyl)-2-methyl-2-propenal was 79.84%.

[0051] Embodiment 12:

[0052] Preparation method of solid high entropy catalyst and its application in catalytic cascade reaction of furfural and n-propanol:

[0053] 0.6g of anhydrous glucose and 0.4g of dodecyltrimethylammonium chloride (DTAC) were added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, V) was added. After being fully stirred for 20min to dissolve, the mixture was ultrasonicated for 2h. The completely dissolved solution was kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst was washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst was obtained by grinding. Take 0.025g of the above catalyst, 0.025g of Cs 2 CO 3 , 0.1 g furfural was added to a polytetrafluoroethylene autoclave, and then 10 mL of n-propanol solvent was added, and 0.3 MPaO 2 , and heated to 130°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 76.4%, and the yield of 3-(2-furanyl)-2-methyl-2-propenal was 73.25%.

[0054] Embodiment 13:

[0055] Preparation method of high solid high entropy catalyst and its application in catalytic series reaction of furfural and n-propanol:

[0056] 0.6g of chitosan and 0.4g of dodecyltrimethylammonium chloride (DTAC) were added to 30mL of oleylamine, and 0.3mmol of acetylacetone metal complex (Fe, Mn, Cu, La, Mg) was added. After fully stirring for 20min to dissolve, the mixture was ultrasonicated for 2h. The completely dissolved solution was kept at 220℃ for 5h to obtain a high entropy catalyst. The high entropy catalyst was washed with a mixture of cyclohexane and ethanol by centrifugation for 3 times, and then dried in a vacuum drying oven at 60℃ overnight. After drying, the high entropy catalyst was obtained by grinding. Take 0.025g of the above catalyst, 0.025g of Cs 2 CO 3 , 0.1 g furfural was added to a polytetrafluoroethylene autoclave, and then 10 mL of n-propanol solvent was added, and 0.3 MPaO 2 , and heated to 130°C with stirring for 2 hours. After the reaction solution was filtered, gas phase analysis showed that the conversion rate of furfural was 58.14% and the yield of 3-(2-furanyl)-2-methyl-2-propenal was 44.52%.

Claims

1. A method for applying a solid high entropy catalyst, characterized in that: The method is applied to the reaction of biomass-based furfural and fatty alcohol selective oxidation-condensation to produce furan acrolein, and the steps are: Biomass-based furfural is used as a reaction substrate, alcohol is used as a solvent, a solid high entropy catalyst is added, an alkali auxiliary is added, heating and stirring are performed, and furfural and fatty alcohol undergo a catalytic series reaction, and the method is carried out using oxygen as an oxidant; The preparation process of the solid high entropy catalyst is: Use 0-1 mol of acetylacetonate metal complex, 0-1 kg of anhydrous glucose, 0-1 kg of dodecyltrimethylammonium chloride (DTAC), and 0-50 L of oleylamine solution, wherein the above four reactants are not 0; fully stir for 20 minutes to dissolve, then ultrasonicate for 2 hours, and keep the completely dissolved solution at 220°C for 5 hours to obtain a high entropy catalyst solution, add a mixed solution of cyclohexane and ethanol to the high entropy catalyst solution, centrifuge and wash 3 times, dry in a vacuum drying oven at 60°C overnight, and grind after drying to obtain a high entropy catalyst; the acetylacetonate metal complex used is five or more of acetylacetonate iron, acetylacetonate manganese, acetylacetonate cobalt, acetylacetonate nickel, acetylacetonate platinum or acetylacetonate aluminum, wherein the above acetylacetonate metal complexes can be replaced by acetylacetonate complexes of metal copper, chromium, vanadium, lanthanum, and cerium.

2. The application method of the solid high entropy catalyst according to claim 1, characterized in that: The fatty alcohol is one or more of ethanol, propanol, isopropanol, butanol, isobutanol, n-pentanol, n-hexanol, n-heptanol, n-octanol or isooctyl alcohol.

3. The application method of the solid high entropy catalyst according to claim 1, characterized in that: The alkali auxiliary agent is one or more of Li2CO3, Na2CO3, K2CO3, Cs2CO3, KHCO3, NaHCO3, LiOH, NaOH, KOH, SrOH, Ca(OH)2, CaO, sodium formate, sodium acetate, sodium propionate, sodium methoxide or sodium ethoxide.

4. The application method of the solid high entropy catalyst according to claim 1, characterized in that: The heating reaction temperature is 80-240°C; the reaction time is 2-60h; the stirring rate is 0-9000r / min, and the stirring rate is not 0.

5. The application method of the solid high entropy catalyst according to claim 1, characterized in that: The mass percentage of the catalyst and the reaction substrate furfural is 0.0001-50%.

6. The application method of the solid high entropy catalyst according to claim 1, characterized in that: The oxygen in the reaction oxidant is replaced by one of air, hydrogen peroxide or tert-butyl hydroperoxide.