A high entropy oxide nanosheet and preparation method thereof
By dispersing metal ions on a water-soluble salt template and utilizing the chelation effect of 1,10-phenanthroline, high-entropy oxide nanosheets were successfully prepared, which solved the problem of difficulty in preparing high-entropy oxide nanosheets in the existing technology. Realizing the advantages of high-entropy oxides in the fields of catalysis and energy storage.
Patent Information
- Application Number
- CN202310224062.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-09
- Filing Date
- 2023-03-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-08
AI Technical Summary
It is difficult to prepare high-entropy oxide nanosheets with existing technology, especially high-entropy oxide nanosheets with non-layered structures, and the co-precipitation method mainly obtains nanoparticle morphology, lacking a universal synthesis method.
Using 1,10-phenanthroline as a chelating agent, the metal ions are evenly dispersed on the water-soluble salt template. Through pressing and heating reactions, the longitudinal growth of the metal oxide is restricted and the lateral growth space is retained. The template is then removed by washing with water to obtain High entropy oxide nanosheets.
Achieved the preparation of high-entropy oxide nanosheets with different structures and components, with two-dimensional morphology and large specific surface area, suitable for catalysis and energy storage fields, low cost, strong universality, simple post-processing, and no additional component residues .
Smart Images

Figure CN116281868B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic chemistry in materials, and in particular to a high entropy oxide nanosheet and a preparation method thereof. Background Art
[0002] Two-dimensional materials have the characteristics of atomic-level thickness (generally <5nm), high specific surface area, and highly exposed surface atoms. Therefore, atomic-level thin nanomaterials are widely used in catalysis, nanoelectronics, sensing, biomedicine, energy storage and conversion, etc. In recent years, two-dimensional materials have been a hot topic of research, but most of them are concentrated in the research of layered structure materials.
[0003] Layered materials have strong chemical bonds in the plane, and are mainly connected by weak interaction forces in the stacking direction. Since the layers of 2D layered materials are connected by weak van der Waals forces, it is easy to obtain single-layer or few-layer nanosheets through mechanical exfoliation, liquid exfoliation, chemical vapor deposition, etc. However, the layers of some non-layered materials are connected by strong chemical bonds, and there is no obvious natural stratification inside the crystal of the material, so two-dimensional materials cannot be obtained by mechanical exfoliation. Compared with 2D layered materials, 2D non-layered materials have the advantages of both atomically thin structure and highly active surface. Therefore, when 3D materials become 2D materials with only a few nanometers of atomic thickness, the lattice structure will be distorted due to the sharp decrease in thickness, and eventually a stable structure with low surface energy will be formed. At the same time, the change in the crystal structure will also cause changes in the energy band structure and electronic state of the material. Secondly, due to the breaking of the vertical chemical bonds of the 3D material, a large number of unsaturated dangling bonds will be generated on the surface of the 2D non-layered material, and the surface polarization will form a large number of active sites and a highly active surface with a large specific surface area. If the 3D bulk material is prepared into a 2D material through some specific methods to fully expose the atoms and active sites of the material, the performance of the material itself can be fully exerted.
[0004] High entropy oxides are non-layered metal oxides that have attracted much attention in recent years. Compared with traditional oxides with few components, high entropy oxides are multi-element oxides that are solid-dissolved into a single structure with five or more elements in an equimolar ratio. In addition to the properties of each main element, they also produce additional properties. Therefore, high entropy oxides have good development potential in basic physics, mechanics, energy storage, and catalysis. At present, people generally use the co-precipitation method to prepare high entropy oxides, but the high entropy oxides obtained by the co-precipitation method are mostly nanoparticles, and there are few reports on the synthesis of high entropy oxide nanosheets.
[0005] Currently, the metal oxide nanosheets synthesized reportedly focus on metal oxides with layered structures. Few articles report the synthesis of non-layered metal oxides with nanosheet morphology. Moreover, only a few single-component metal oxide nanosheets can be prepared, and the synthesis methods are not universal. Summary of the invention
[0006] Based on this, an embodiment of the present invention provides a high entropy oxide nanosheet and a preparation method thereof. The preparation method can synthesize high entropy oxide nanosheets with different structures and different components, has simple post-processing and strong universality.
[0007] To achieve the above object, on the one hand, an embodiment of the present invention provides a method for preparing a high entropy oxide nanosheet, comprising the following steps:
[0008] SO1, dissolving 1,10-phenanthroline in a first organic solution to obtain a 1,10-phenanthroline solution; adding a water-soluble salt to the 1,10-phenanthroline solution, stirring evenly, to obtain a first mixed solution;
[0009] SO2, adding the reactant to the second organic solution to obtain a reactant solution; adding the reactant solution to the first mixed solution of step S01, stirring evenly, to obtain a second mixed solution;
[0010] SO3, filtering the second mixed solution in step S02, taking the filter residue, and vacuum drying to obtain a precursor; pressing the precursor to obtain a precursor wafer;
[0011] SO4, in an air atmosphere, heating the precursor wafer of step S03 to react to obtain a first product;
[0012] SO5. Wash the first product of step SO4 with water to obtain a water wash liquid; filter the water wash liquid, take the filter residue, wash with ethanol to obtain an ethanol wash liquid; filter the ethanol wash liquid, take the filter residue, and vacuum dry to obtain high entropy oxide nanosheets.
[0013] As a preferred embodiment, in step SO1,
[0014] The ratio of the mass of the water-soluble salt to the volume of the first organic solution is (1-2) g: (0.5-3) ml.
[0015] The water-soluble salt is a metal salt that is soluble in water but insoluble in an organic solvent.
[0016] The particle size of the water-soluble salt is 10 μm to 50 μm.
[0017] The stirring time is 2h to 6h.
[0018] The first organic solution is preferably an anhydrous ethanol solution or an acetone solution.
[0019] As a preferred embodiment, in step SO2,
[0020] The molar ratio of the reactant to the 1,10-phenanthroline in step SO1 is 1 mol:(1-2) mol.
[0021] The mass ratio of the reactant to the water-soluble salt of step SO1 is 1 g:(200-400) g.
[0022] The ratio of the mass of the reactant to the volume of the second organic solution is (0.05-0.2) g: (3-6) ml.
[0023] The reactants are one or at least two metal salts soluble in organic solutions. When the reactants are at least two metal salts soluble in organic solutions, the reactants are added sequentially, one reactant is added at a time, and the interval between two adjacent additions is 5 minutes to 30 minutes.
[0024] The stirring time is 2h to 12h.
[0025] The second organic solution is preferably an anhydrous ethanol solution or an acetone solution.
[0026] As a preferred embodiment, in step SO3,
[0027] The vacuum drying is performed at 60° C. to 80° C. for 6 h to 12 h.
[0028] The pressing is achieved by using a tabletting die; the pressing pressure is 5Mpa to 15Mpa; the precursor disc is a disc with a diameter of 18mm and a thickness of (0.1 to 0.2)mm.
[0029] As a preferred embodiment, in step SO4,
[0030] The heating reaction is carried out at 150° C. to 850° C. for 15 min to 300 min.
[0031] As a preferred embodiment, in step SO5,
[0032] The number of times of water washing is 3 to 6 times, and the number of times of ethanol washing is 2 to 3 times.
[0033] The vacuum drying is performed at 60° C. to 80° C. for 6 h to 12 h.
[0034] On the other hand, an embodiment of the present invention also provides a high entropy oxide nanosheet obtained by the above preparation method.
[0035] Compared with the prior art, this application has the following technical effects:
[0036] (1) The present invention uses a chelating agent 1,10-phenanthroline to uniformly disperse a small amount of metal ions on a large amount of water-soluble salt templates to obtain a precursor, and then presses the precursor into sheets, reacts at a suitable temperature for a period of time, and limits the longitudinal growth of metal oxides through a large amount of water-soluble salt templates and retains lateral growth space. The water-soluble salt templates are washed away with water to obtain high entropy oxide nanosheets.
[0037] (2) The preparation method of the present application can prepare mono- or poly-layered and non-layered metal oxide nanosheets. The preparation method has low cost, strong universality, simple post-processing, and no additional components remain. In addition to synthesizing high entropy oxide nanosheets containing five elements or more single structures, mono- or poly-layered and non-layered metal oxide nanosheets can also be prepared.
[0038] (3) Compared with high entropy oxide nanoparticles, the high entropy oxide nanosheets prepared in the present application have a two-dimensional morphology. The two-dimensional morphology with a large specific surface area can expose more surface atoms, making the high entropy oxide with a two-dimensional sheet morphology more advantageous in the fields of catalysis and energy storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 is the XRD characterization diagram of the Fe2O3 two-dimensional sheet prepared in Example 1;
[0041] Figure 2 is a SEM characterization image of the Fe2O3 two-dimensional sheet prepared in Example 1;
[0042] Figure 3 The Na obtained in Example 2 0.13 V 0.13 Mo 0.87 XRD characterization of O3 two-dimensional sheet;
[0043] Figure 4 The Na obtained in Example 2 0.13 V 0.13 Mo 0.87 SEM characterization of O3 two-dimensional sheet;
[0044] Figure 5is the XRD characterization diagram of the (MgCoNiCuZn)O two-dimensional sheet prepared in Example 3;
[0045] Figure 6 is a SEM characterization image of the (MgCoNiCuZn)O two-dimensional sheet prepared in Example 3;
[0046] Figure 7 This is the XRD characterization diagram of the (CrFeMnCoNi)3O4 two-dimensional sheet prepared in Example 4;
[0047] Figure 8 This is the SEM characterization image of the (CrFeMnCoNi)3O4 two-dimensional sheet prepared in Example 4.
[0048] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0049] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, top, bottom...), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0051] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0052] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0053] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0054] At present, people generally use the coprecipitation method to synthesize high entropy oxides, but the high entropy oxides obtained by the coprecipitation method are mostly in the form of nanoparticles, and other synthesis methods are rarely reported to synthesize high entropy oxide nanosheets. Based on this, it is necessary to provide a high entropy oxide nanosheet and a preparation method thereof to solve the above technical problems.
[0055] To achieve the above object, on the one hand, an embodiment of the present invention provides a method for preparing a high entropy oxide nanosheet, comprising the following steps:
[0056] SO1, dissolving 1,10-phenanthroline in a first organic solution to obtain a 1,10-phenanthroline solution; adding a water-soluble salt (serving as a reactant template) to the 1,10-phenanthroline solution, stirring evenly, to obtain a first mixed solution;
[0057] SO2, adding the reactant to the second organic solution to obtain a reactant solution; adding the reactant solution to the first mixed solution of step S01, stirring evenly, to obtain a second mixed solution;
[0058] SO3, filtering the second mixed solution in step S02, taking the filter residue, and vacuum drying to obtain a precursor; pressing the precursor to obtain a precursor wafer;
[0059] SO4, in an air atmosphere, heating the precursor wafer of step S03 to react to obtain a first product;
[0060] SO5. Wash the first product of step SO4 with water (dissolve and remove soluble salts) to obtain a water wash solution; filter the water wash solution, take the filter residue, wash with ethanol to obtain an ethanol wash solution; filter the ethanol wash solution, take the filter residue, and vacuum dry to obtain high entropy oxide nanosheets.
[0061] As a preferred embodiment, in step SO1,
[0062] The ratio of the mass of the water-soluble salt to the volume of the first organic solution is (1-2) g: (0.5-3) ml. In this way, the longitudinal growth of the metal oxide can be limited by a large amount of water-soluble salt templates, and the lateral growth space can be reserved.
[0063] The water-soluble salt is a metal salt that is soluble in water but insoluble in an organic solvent, preferably NaCl.
[0064] The particle size of the water-soluble salt is 10 μm to 50 μm.
[0065] The stirring time is 2h to 6h.
[0066] Specifically, in this embodiment, the first organic solution is an anhydrous ethanol solution or an acetone solution. In other embodiments, the first organic solution can also be replaced by other organic solvents that have higher solubility for the reactants.
[0067] As a preferred embodiment, in step SO2,
[0068] The molar ratio of the reactant to the 1,10-phenanthroline in step SO1 is 1 mol:(1-2) mol.
[0069] The mass ratio of the reactant to the water-soluble salt in step SO1 is 1 g: (200-400) g. In this way, the longitudinal growth of the metal oxide can be limited by a large amount of water-soluble salt templates, and the lateral growth space can be reserved; at the same time, the generation of high entropy oxide nanosheets can be well guaranteed.
[0070] The ratio of the mass of the reactant to the volume of the second organic solution is (0.05-0.2) g: (3-6) ml. In this way, the generation of high entropy oxide nanosheets can be well guaranteed.
[0071] The reactants are one or at least two metal salts soluble in an organic solution, preferably one or at least two metal salts such as nitrates, chlorides and carbonates (such as CoCl2, NiCl2, CuCl2 and ZnCl2, etc.); when the reactants are at least two metal salts soluble in an organic solution, the reactants are added sequentially, one reactant is added at a time, and the interval between two adjacent additions is 5 minutes to 30 minutes.
[0072] The stirring time is 2h to 12h.
[0073] Specifically, in the embodiment of the present application, the second organic solution is an anhydrous ethanol solution or an acetone solution. In other embodiments, the second organic solution can also be replaced by other organic solvents that have a higher solubility for the reactants.
[0074] As a preferred embodiment, in step SO3,
[0075] The vacuum drying is performed at 60° C. to 80° C. for 6 h to 12 h.
[0076] The pressing is achieved by using a tabletting die; the pressing pressure is 5Mpa to 15Mpa; the precursor disc is a disc with a diameter of 18mm and a thickness of (0.1 to 0.2)mm.
[0077] As a preferred embodiment, in step SO4,
[0078] The heating reaction is carried out at 150° C. to 850° C. for 15 min to 300 min.
[0079] As a preferred embodiment, in step SO5,
[0080] The number of times of water washing is 3 to 6 times, and the number of times of ethanol washing is 2 to 3 times.
[0081] The vacuum drying is performed at 60° C. to 80° C. for 6 h to 12 h.
[0082] On the other hand, an embodiment of the present invention also provides a high entropy oxide nanosheet obtained by the above preparation method.
[0083] Compared with the prior art, this application has the following technical effects:
[0084] (1) The present invention uses a chelating agent 1,10-phenanthroline to uniformly disperse a small amount of metal ions on a large amount of water-soluble salt templates to obtain a precursor, and then presses the precursor into sheets, reacts at a suitable temperature for a period of time, and limits the longitudinal growth of metal oxides through a large amount of water-soluble salt templates and retains lateral growth space. The water-soluble salt templates are washed away with water to obtain high entropy oxide nanosheets.
[0085] (2) The preparation method of the present application can prepare mono- or poly-layered and non-layered metal oxide nanosheets. The preparation method has low cost, strong universality, simple post-processing, and no additional components remain. In addition to synthesizing high entropy oxide nanosheets, mono- or poly-layered and non-layered metal oxide nanosheets can also be prepared.
[0086] (3) Compared with high entropy oxide nanoparticles, the high entropy oxide nanosheets prepared in the present application have a two-dimensional morphology. The two-dimensional morphology with a large specific surface area can expose more surface atoms, making the high entropy oxide with a two-dimensional sheet morphology more advantageous in the fields of catalysis and energy storage.
[0087] Example 1
[0088] A method for preparing a high entropy oxide nanosheet (Fe2O3 two-dimensional sheet) comprises the following steps:
[0089] SO1, dissolving 0.108 g of 1,10-phenanthroline in 20 ml of anhydrous ethanol solution to obtain a 1,10-phenanthroline solution; adding 20 g of NaCl to the 1,10-phenanthroline solution and stirring evenly to obtain a first mixed solution;
[0090] SO2, adding 0.176g of ferric acetylacetonate to 5ml of anhydrous ethanol solution to obtain a reactant solution; adding the reactant solution to the first mixed solution of step S01, stirring evenly, to obtain a second mixed solution;
[0091] SO3, filtering the second mixed solution in step S02, taking the filter residue, and vacuum drying to obtain a precursor; pressing the precursor to obtain a precursor wafer;
[0092] SO4, in an air atmosphere, heating the precursor wafer of step S03 to react to obtain a first product;
[0093] SO5. Wash the first product of step SO4 with water to obtain a water wash liquid; filter the water wash liquid, take the filter residue, wash with ethanol to obtain an ethanol wash liquid; filter the ethanol wash liquid, take the filter residue, and vacuum dry to obtain high entropy oxide nanosheets.
[0094] In step SO1,
[0095] The particle size of the water-soluble salt is 10 μm to 50 μm.
[0096] The stirring time is 2h.
[0097] In step SO2,
[0098] The stirring (magnetic stirring) time is 6 hours.
[0099] In step SO3,
[0100] The vacuum drying is performed at 60° C. for 12 h.
[0101] The pressing is achieved by using a tabletting mold; the pressing pressure is 15 MPa; the precursor disc is a disc with a diameter of 18 mm and a thickness of 0.2 mm.
[0102] In step SO4,
[0103] The heating reaction is carried out at 180° C. for 180 min.
[0104] In step SO5,
[0105] The water washing was performed 3 times, and the ethanol washing was performed 2 times.
[0106] The vacuum drying is performed at 60° C. for 12 h.
[0107] Figure 1 and Figure 2 They are respectively the XRD and SEM images of the Fe2O3 two-dimensional sheet prepared in Example 1; the XRD image shows that pure phase Fe2O3 is generated in this example, and the SEM image shows that the Fe2O3 has an obvious flaky morphology.
[0108] Example 2
[0109] A high entropy oxide nanosheet (Na 0.13 V 0.13 Mo 0.87 A method for preparing an O3 two-dimensional sheet) comprises the following steps:
[0110] SO1, dissolving 0.022g of 1,10-phenanthroline in 20ml of acetone solution to obtain a 1,10-phenanthroline solution; adding 20g of NaCl to the 1,10-phenanthroline solution and stirring evenly to obtain a first mixed solution;
[0111] SO2, dissolving 0.02g of vanadium acetylacetonate and 0.02g of molybdenum acetylacetonate in 5ml of acetone solution to obtain a reactant solution; adding the reactant solution to the first mixed solution of step S01 (using a method of adding reactants in sequence, adding one reactant solution at a time, and adding intervals of 30min), stirring evenly to obtain a second mixed solution;
[0112] SO3, filtering the second mixed solution in step S02, taking the filter residue, and vacuum drying to obtain a precursor; pressing the precursor to obtain a precursor wafer;
[0113] SO4, in an air atmosphere, heating the precursor wafer of step S03 to react to obtain a first product;
[0114] SO5. Wash the first product of step SO4 with water to obtain a water wash liquid; filter the water wash liquid, take the filter residue, wash with ethanol to obtain an ethanol wash liquid; filter the ethanol wash liquid, take the filter residue, and vacuum dry to obtain high entropy oxide nanosheets.
[0115] In step SO1,
[0116] The particle size of the water-soluble salt is 10 μm to 50 μm.
[0117] The stirring time is 2h.
[0118] In step SO2,
[0119] The stirring (magnetic stirring) time is 6 hours.
[0120] In step SO3,
[0121] The vacuum drying is performed at 60° C. for 12 h.
[0122] The pressing is achieved by using a tabletting mold; the pressing pressure is 10 MPa; the precursor disc is a disc with a diameter of 18 mm and a thickness of 0.2 mm.
[0123] In step SO4,
[0124] The heating reaction is carried out at 170° C. for 180 min.
[0125] In step SO5,
[0126] The water washing was performed 3 times, and the ethanol washing was performed 2 times.
[0127] The vacuum drying is performed at 60° C. for 12 h. Figure 3 and Figure 4 The obtained Na 0.13 V 0.13 Mo 0.87 XRD and SEM images of O3 two-dimensional sheets; XRD images show that pure phase Na 0.13 V 0.13 Mo 0.87 O3 two-dimensional sheet, from the SEM image we can see Na 0.13 V 0.13 Mo 0.87 O3 two-dimensional sheets have obvious flake morphology.
[0128] Example 3
[0129] A method for preparing a high entropy oxide nanosheet ((MgCoNiCuZn)O two-dimensional sheet) comprises the following steps:
[0130] SO1, dissolving 0.5 g of 1,10-phenanthroline in 80 ml of anhydrous ethanol solution to obtain a 1,10-phenanthroline solution; adding 100 g of NaCl to the 1,10-phenanthroline solution and stirring to obtain a first mixed solution;
[0131] SO2, dissolve 0.0004 mol of MgCl2 (0.0813 g), CoCl2 (0.0519 g), NiCl2 (0.0951 g), CuCl2 (0.0537 g), and ZnCl2 (0.0545 g) in 5 ml of anhydrous ethanol solution to obtain a reactant solution; add the reactant solution to the first mixed solution of step S01 (adopting a method of adding reactants in sequence, adding one reactant solution at a time, and adding intervals of 30 minutes), stir evenly, and obtain a second mixed solution;
[0132] SO3, filtering the second mixed solution in step S02, taking the filter residue, and vacuum drying to obtain a precursor; pressing the precursor to obtain a precursor wafer;
[0133] SO4, in an air atmosphere, heating the precursor wafer of step S03 to react to obtain a first product;
[0134] SO5. Wash the first product of step SO4 with water to obtain a water wash liquid; filter the water wash liquid, take the filter residue, wash with ethanol to obtain an ethanol wash liquid; filter the ethanol wash liquid, take the filter residue, and vacuum dry to obtain high entropy oxide nanosheets.
[0135] In step SO1,
[0136] The particle size of the water-soluble salt is 10 μm to 50 μm.
[0137] The stirring time is 6 hours.
[0138] In step SO2,
[0139] The stirring (magnetic stirring) time is 12h.
[0140] In step SO3,
[0141] The vacuum drying is performed at 60° C. for 12 h.
[0142] The pressing is achieved by using a tabletting mold; the pressing pressure is 5 MPa; the precursor disc is a disc with a diameter of 18 mm and a thickness of 0.2 mm.
[0143] In step SO4,
[0144] The heating reaction is carried out at 800° C. for 60 minutes.
[0145] In step SO5,
[0146] The water washing was performed 3 times, and the ethanol washing was performed 2 times.
[0147] The vacuum drying is performed at 60° C. for 12 h.
[0148] Figure 5 and Figure 6 They are XRD and SEM images of the (MgCoNiCuZn)O two-dimensional sheet prepared in Example 4. The XRD image shows that pure phase (MgCoNiCuZn)O is generated in this example. The SEM image shows that (MgCoNiCuZn)O has obvious flaky morphology.
[0149] Example 4
[0150] A method for preparing a high entropy oxide nanosheet ((CrFeMnCoNi)3O4 two-dimensional sheet) comprises the following steps:
[0151] SO1, dissolving 0.5 g of 1,10-phenanthroline in 50 ml of anhydrous ethanol solution to obtain a 1,10-phenanthroline solution; adding 50 g of NaCl to the 1,10-phenanthroline solution and stirring evenly to obtain a first mixed solution;
[0152] SO2, dissolve 0.0004 mol of Cr(NO3)3.9H2O (0.160 g), Fe(NO3)3 (0.097 g), Mn(NO3)2.4H2O (0.096 g), Co(NO3)2.6H2O (0.116 g), and Ni(NO3)2.6H2O (0.116 g) in 5 ml of anhydrous ethanol solution to obtain a reactant solution; add the reactant solution to the first mixed solution of step S01 (add the reactants in sequence, one reactant solution at a time, with an interval of 5 minutes), stir evenly, and obtain a second mixed solution;
[0153] SO3, filtering the second mixed solution in step S02, taking the filter residue, and vacuum drying to obtain a precursor; pressing the precursor to obtain a precursor wafer;
[0154] SO4, in an air atmosphere, heating the precursor wafer of step S03 to react to obtain a first product;
[0155] SO5. Wash the first product of step SO4 with water to obtain a water wash liquid; filter the water wash liquid, take the filter residue, wash with ethanol to obtain an ethanol wash liquid; filter the ethanol wash liquid, take the filter residue, and vacuum dry to obtain high entropy oxide nanosheets.
[0156] In step SO1,
[0157] The particle size of the water-soluble salt is 10 μm to 50 μm.
[0158] The stirring time is 6 hours.
[0159] In step SO2,
[0160] The stirring (magnetic stirring) time is 12h.
[0161] In step SO3,
[0162] The vacuum drying is performed at 60° C. for 12 h.
[0163] The pressing is achieved by using a tabletting mold; the pressing pressure is 5 MPa; the precursor disc is a disc with a diameter of 18 mm and a thickness of 0.2 mm.
[0164] In step SO4,
[0165] The heating reaction is carried out at 800° C. for 60 minutes.
[0166] In step SO5,
[0167] The water washing was performed 3 times, and the ethanol washing was performed 2 times.
[0168] The vacuum drying is performed at 60° C. for 12 h.
[0169] Figure 7 and Figure 8 They are XRD and SEM images of the (CrFeMnCoNi)3O4 two-dimensional sheet prepared in Example 4. The XRD image shows that pure phase (CrFeMnCoNi)3O4 is generated in this example. From the SEM image, it can be seen that (CrFeMnCoNi)3O4 has obvious flaky morphology.
[0170] Comparative Example 1
[0171] Reference for this comparative example: Xiao, X., Song, H., Lin, S. et al. Scalable salt-templated synthesis of two-dimensional transition metal oxides. Nat Commun 7, 11296 (2016).
[0172] The preparation process is as follows:
[0173] (1) Disperse 0.1 g Mo powder in 20 ml ethanol and stir for 30 min to obtain a Mo powder suspension;
[0174] (2) Slowly add 0.35 ml of H2O2 (30%) to the Mo powder suspension in step (1) and stir for 18 h to obtain a precursor solution;
[0175] (3) adding 320 g of NaCl to the above precursor solution, stirring and drying at 65° C. to obtain a sample;
[0176] (4) In an Ar atmosphere, the obtained sample was heated at 2 °C min -1 The reaction was carried out at a heating rate of 500 °C for 1 h, cooled, and the NaCl template was removed with deionized water. The reaction was dried to obtain MoO2.
[0177] Comparative Example 1 and the method of the present invention both use soluble salts as templates to assist in the synthesis of two-dimensional materials. The materials synthesized in Comparative Example 1 are mainly mono-metallic oxide nanosheets, but the method of the present invention can synthesize mono- to poly-laminated and non-laminated metal oxide nanosheets, and any metal oxide that meets the synthesis conditions of the method can be synthesized, and the method is more universal.
[0178] Comparative Example 2
[0179] Reference for this comparative example: Wu H, Lu Q, Wang J. et al. Rapid Joule-Heating Synthesis for Manufacturing High-Entropy Oxides as Efficient Electrocatalysts. NanoLett. 2022, 22, 6492-6500.
[0180] The preparation process is as follows:
[0181] (1) synthesizing a hydroxide precursor by a coprecipitation method, dissolving 0.8 mmol Mg(NO3)2.6H2O, 0.8 mmol FeSO4.7H2O, 0.8 mmol Co(NO3)2.6H2O, 0.8 mmol Ni(NO3)2.6H2O, and 0.8 mmol Zn(NO3)2.6H2O in 50 ml of water to obtain a salt solution;
[0182] (2) then dripping the above salt solution and 1 M KOH into 50 ml of 0.1 M KOH solution simultaneously, adjusting the dripping rate so that the pH is always maintained at 13, until the salt solution is consumed to obtain a hydroxide precipitate;
[0183] (3) centrifuging the hydroxide precipitate, washing with deionized water and ethanol in sequence, and drying under vacuum at 60° C. to obtain a sample;
[0184] (4) In an Ar atmosphere, a current of 30 A was passed for 30 s to heat the nickel foil containing the sample to obtain a high entropy oxide (MgFeCoNiZn)O.
[0185] Comparative Example 2 uses a coprecipitation method to rapidly heat up and synthesize a high entropy oxide, and the high entropy oxides synthesized by this method are mostly in the form of nanoparticles. The present invention successfully synthesizes high entropy oxide nanosheets by using a salt template confined growth method, and can synthesize high entropy oxides in a variety of nanosheet morphologies. The method is simple and easy to implement and has strong universality.
[0186] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing high entropy oxide nanosheets, characterized in that: The steps include: S01, dissolving 1,10-phenanthroline in a first organic solution to obtain a 1,10-phenanthroline solution; adding a water-soluble salt to the 1,10-phenanthroline solution, stirring evenly, to obtain a first mixed solution; S02, adding the reactant to the second organic solution to obtain a reactant solution; Adding the reactant solution to the first mixed solution in step S01 and stirring evenly to obtain a second mixed solution; S03, filtering the second mixed solution in step S02, taking the filter residue, and vacuum drying to obtain a precursor; Pressing the precursor to obtain a precursor wafer; S04, heating the precursor wafer in step S03 in an air atmosphere to obtain a first product; S05, washing the first product of step S04 with water to obtain a washing liquid; The water washing liquid is filtered, the filter residue is taken, and the residue is washed with ethanol to obtain an ethanol washing liquid; the ethanol washing liquid is filtered, the filter residue is taken, and vacuum drying is performed to obtain a high entropy oxide nanosheet; The high entropy oxide nanosheet is a high entropy oxide nanosheet with a two-dimensional sheet morphology; The water-soluble salt is a metal salt that is soluble in water but insoluble in organic solvents; The reactant is one or at least two metal salts soluble in an organic solution; when the reactant is at least two metal salts soluble in an organic solution, the reactants are added sequentially, one reactant is added at a time, and the interval between the two adjacent additions is 5min to 30min; In step S01, the ratio of the mass of the water-soluble salt to the volume of the first organic solution is (1-2) g: (0.5-3) ml; In step S02, the molar ratio of the reactant to the 1,10-phenanthroline in step S01 is 1 mol:(1-2) mol; In step S02, the mass ratio of the reactant to the water-soluble salt in step S01 is 1 g:(200-400) g.
2. The method for preparing high entropy oxide nanosheets according to claim 1, characterized in that: In step S01, the particle size of the water-soluble salt is 10 μm to 50 μm; The stirring time is 2h to 6h; The first organic solution is an anhydrous ethanol solution or an acetone solution.
3. The method for preparing high entropy oxide nanosheets according to claim 1, characterized in that: In step S02, the ratio of the mass of the reactant to the volume of the second organic solution is (0.05-0.2) g: (3-6) ml.
4. The method for preparing high entropy oxide nanosheets according to claim 1, characterized in that: In step S02, the stirring time is 2h to 12h; The second organic solution is an anhydrous ethanol solution or an acetone solution.
5. The method for preparing high entropy oxide nanosheets according to claim 1, characterized in that: In step S03, The vacuum drying is performed at 60°C to 80°C for 6h to 12h; The pressing is achieved by using a tabletting die; the pressing pressure is 5Mpa to 15Mpa; the precursor disc is a disc with a diameter of 18mm and a thickness of (0.1 to 0.2)mm.
6. The method for preparing high entropy oxide nanosheets according to claim 1, characterized in that: In step S04, the heating reaction is carried out at 150°C to 850°C for 15min to 300min; In step S05, the vacuum drying is performed at 60°C to 80°C for 6h to 12h.