A preparation method and drawing device of three-dimensional graphene, and application thereof

Through the reduction treatment and plastic stretching of three-dimensional graphene oxide, a wrinkled morphology is constructed and its conductive mode is transformed into a metallic type. This solves the problem of temperature dependence of the conductivity of three-dimensional graphene and realizes the transport and retention of metallic-type carriers. mechanical properties.

CN116281986BActive Publication Date: 2024-10-29HUANENG RENEWABLES CORPORATION LIMITED +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310407589.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

The conductivity of three-dimensional graphene has a typical "insulating" temperature dependence, and it is difficult to achieve a metallic carrier transport mode when the carrier concentration is high, limiting its application in the field of high-power electronic devices.

Method used

By performing the first reduction treatment, plastic drawing and second reduction treatment on the sheet-like three-dimensional graphene oxide, more wrinkled morphologies are constructed, its conductive mode is transformed into a metallic type, and the energy band structure is transformed from a band gap open type. It is a bandgap overlapping type.

Benefits of technology

Successfully reduced the conductivity of three-dimensional graphene as the temperature increases, achieving a metallic carrier transport mode, avoiding the inconvenience of traditional doping technology, while retaining the mechanical performance advantages of graphene, such as light weight and high strength , flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116281986B_ABST
    Figure CN116281986B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of graphene technology, and specifically provides a method for preparing three-dimensional graphene, a stretching device, and an application thereof. The method for preparing three-dimensional graphene of the present invention comprises: (1) performing a first reduction treatment on flaky three-dimensional graphene oxide to obtain a first intermediate product; (2) stretching the first intermediate product to obtain a second intermediate product; (3) performing a second reduction treatment on the second intermediate product to obtain three-dimensional graphene. Compared with the prior art, the method of the present invention constructs more wrinkled morphologies on the surface of three-dimensional graphene through plastic stretching and reduction treatment, thereby transforming its conductive mode from semiconductor type to metal type, while retaining the inherent mechanical performance advantages of graphene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of graphene, and more specifically, to a preparation method, a drawing device and an application of three-dimensional graphene. Background Art

[0002] Graphene is a sp 2 Carbon atoms connected by orbital hybridization are stacked into a single-layer two-dimensional honeycomb lattice structure. Graphene has a unique "Dirac cone" band structure, which makes it have an extremely high carrier mobility of about 1000cm at room temperature. 2 ·V -1 ·s. In addition, graphene has mechanical characteristics such as flexibility, light weight, high strength and flexible processing, providing a highly promising alternative for the research and development and manufacturing of semiconductor electronic devices in the "post-silicon" era. However, the unique zero-gap Dirac cone band structure of graphene has greatly limited its application in the preparation of semiconductor electronic devices. The two-dimensional morphology of graphene still faces many challenges in large-scale preparation and application. In addition, the low-dimensional morphology of graphene leads to its insufficient specific capacity, which greatly limits its application in many fields such as the field of high-power electronic devices. The concept of "all-carbon electronics" represented by three-dimensional graphene oxide structures with self-supporting configurations provides a feasible solution to the above problems. Among them, the most representative three-dimensional graphene oxides are graphene sponges, graphene networks and graphene films.

[0003] At present, the conductivity of three-dimensional graphene oxide represented by graphene sponge, graphene network and graphene film has a typical "insulating" temperature dependence. In addition, the "insulating" temperature dependence exists not only at the charge neutral point, but also when the carrier concentration is as high as 10 19 cm -3 The same phenomenon can be observed in the doped system.

[0004] For graphene with a three-dimensional spatial configuration, its internal carriers usually exhibit semiconductor-type transport characteristics, that is, the conductivity shows an increasing trend with increasing temperature. How to realize the metallic carrier transport mode in three-dimensional graphene, that is, the conductivity shows a decreasing trend with increasing temperature, is extremely urgent. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a preparation method and a stretching device and application of three-dimensional graphene, which constructs more wrinkled morphologies on the surface of three-dimensional graphene to transform its conductive mode from semiconductor type to metallic type, that is, the conductivity decreases with increasing temperature, while retaining the inherent mechanical properties advantages of graphene.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing three-dimensional graphene, comprising:

[0008] (1) performing a first reduction treatment on the flaky three-dimensional graphene oxide to obtain a first intermediate product;

[0009] (2) stretching the first intermediate product to obtain a second intermediate product;

[0010] (3) The second intermediate product is subjected to a second reduction treatment to obtain three-dimensional graphene.

[0011] In the present invention, the first reduction treatment specifically comprises: mixing the flaky three-dimensional graphene oxide with a reducing agent solution;

[0012] The second reduction treatment specifically comprises: mixing the second intermediate product with a reducing agent solution.

[0013] In the present invention, the stretching is carried out in a reducing agent solution; the stretching is specifically as follows: the first intermediate product is sequentially wrapped and contacted with the stretching shaft; the rotation speed of the stretching shaft increases along the forward direction of the second intermediate product; the number of the stretching shafts is ≥2.

[0014] In the present invention, the linear speed difference between two adjacent drafting shafts is 0.2 to 0.3 rpm.

[0015] In the present invention, the preparation method further comprises: heat treating the second intermediate product after the second reduction treatment; the temperature of the heat treatment is 2500-3500K.

[0016] In the step (1) of the present invention, the mixing time is 3 to 5 minutes; the stretching time is 15 to 30 seconds; and in the step (3), the mixing time is 3 to 5 minutes.

[0017] The present invention also provides a drafting device, comprising: a drafting trough for accommodating a reducing agent solution; a drafting shaft arranged along the advancing direction of the object to be drafted; and the number of the drafting shafts is ≥2.

[0018] In the present invention, the rotation speed of the drafting shaft increases gradually along the advancing direction of the drafted object.

[0019] The present invention also provides the use of the three-dimensional graphene in preparing materials with metallic carrier characteristics.

[0020] The present invention provides a method for in-situ triggering a metallic carrier transport mode in three-dimensional graphene oxide. The method constructs more wrinkled morphologies of a "percolation network" configuration on the surface of three-dimensional graphene through plastic stretching and reduction treatment, and the wrinkled morphology on the surface of three-dimensional graphene can realize a metallic carrier transport mode, that is, the energy band structure is transformed from a band gap open type to a band gap overlapping type. It is confirmed by the embodiments of the present invention that after the three-dimensional graphene oxide is treated by a method including liquid phase reduction and plastic stretching, the conductivity decreases with the increase of temperature, from 2.7 to 3.4 (100K) to 1.7 to 2.2 (300K).

[0021] The present invention provides a method for in-situ triggering of a metallic carrier transport mode in three-dimensional graphene oxide, which can avoid the inconvenience of executing traditional doping technologies such as element doping and field effect doping, and achieve regulation of local micro-regions and global carrier transport modes; in addition, the three-dimensional graphene containing a wrinkled morphology still retains the inherent mechanical properties advantages of graphene, such as light weight, high strength, flexibility, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of a plasticizing and stretching device according to an embodiment of the present invention, the device is composed of a roller device and a liquid working medium tank, wherein the roller device includes a driving roller 1, a driving roller 2, a transmission roller 1 and a transmission roller 2;

[0023] Figure 2 This is a scanning electron microscope image of three-dimensional graphene according to Example 1 of the present invention;

[0024] Figure 3 This is a graph showing the relationship between conductivity and temperature of Example 1 of the present invention;

[0025] Figure 4 This is a scanning electron microscope image of three-dimensional graphene according to Example 2 of the present invention;

[0026] Figure 5 is a graph showing the relationship between conductivity and temperature of Example 2 of the present invention;

[0027] Figure 6 This is a scanning electron microscope image of three-dimensional graphene according to Example 3 of the present invention;

[0028] Figure 7 This is a graph showing the relationship between conductivity and temperature in Example 3 of the present invention. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention adopts the following technical solutions:

[0031] A method for preparing three-dimensional graphene, comprising:

[0032] (1) performing a first reduction treatment on the flaky three-dimensional graphene oxide to obtain a first intermediate product;

[0033] (2) stretching the first intermediate product to obtain a second intermediate product;

[0034] (3) The second intermediate product is subjected to a second reduction treatment to obtain three-dimensional graphene.

[0035] In the present invention, the first reduction treatment is specifically: mixing the flaky three-dimensional graphene oxide with a reducing agent solution; the mixing time is 3 to 5 minutes, preferably 3 minutes;

[0036] The second reduction treatment specifically comprises: mixing the second intermediate product with a reducing agent solution; the mixing time is 3 to 5 minutes, preferably 3 minutes.

[0037] In the present invention, the stretching is carried out in a reducing agent solution; the stretching time is 5 to 30 seconds; the stretching time is preferably 5 seconds, and after the stretching is completed, the state is maintained for 10 seconds; the stretching is specifically: the first intermediate product is sequentially wrapped and contacted with the stretching shaft; the rotation speed of the stretching shaft increases along the forward direction of the second intermediate product; the number of the stretching shafts is ≥2.

[0038] In the present invention, the linear speed difference between two adjacent drafting shafts is 0.2 to 0.3 rpm.

[0039] In the present invention, the reducing agent solution is obtained by mixing a reducing agent and a solvent; the solvent is an organic solvent; the molecular weight of the reducing agent is ≤500; the reducing agent is preferably hydrogen iodide; in one embodiment of the present invention, the reducing agent solution is a hydrogen iodide solution, and the hydrogen iodide solution is obtained by mixing ethanol and hydrogen iodide; the volume ratio of ethanol to hydrogen iodide is (1-4):1, preferably 1:1.

[0040] In the present invention, the preparation method further comprises: heat treating the second intermediate product after the second reduction treatment; the temperature of the heat treatment is 2500-3500K, preferably 2500K; the time of the heat treatment is preferably 5-8h, preferably 5h.

[0041] In the present invention, the mass ratio of the three-dimensional graphene oxide to the reducing agent solution is 1:(1-100); the mass ratio of the second intermediate product to the reducing agent solution is 1:(1-100).

[0042] The present invention also provides a stretching device, comprising: a stretching trough for accommodating a reducing agent solution; a stretching shaft arranged along the advancing direction of the stretched object; the number of the stretching shafts is ≥2, preferably 2.

[0043] In the present invention, the drafting shaft can be arranged in the drafting groove or outside the drafting groove. When the drafting shaft is arranged outside the drafting groove, the drafting device also includes a transmission shaft arranged in the drafting groove; the number of the transmission shafts is preferably 2.

[0044] In the present invention, the rotation speed of the drafting shaft increases along the advancing direction of the drafted object; and the linear speed difference between two adjacent drafting shafts is 0.2-0.3 rpm.

[0045] In one embodiment of the present invention, the drafting device is composed of a drafting groove and four rollers, and the rollers arranged along the direction of the drafted object are: a driving roller 1, a transmission roller 1, a transmission roller 2 and a driving roller 2, as shown in FIG. Figure 1 As shown, the drafting tank is filled with a reducing agent solution, the transmission roller 1 and the transmission roller 2 are immersed in the liquid working medium, the driving roller 1 and the driving roller 2 are outside the drafting tank, the driving roller 1 and the driving roller 2 are the drafting shafts, the rotation speed of the driving roller 1 is V0, and the rotation speed of the driving roller 2 is V1; V1-V0=0.25 rpm.

[0046] The present invention has no special requirements for three-dimensional graphene oxide, and conventional methods in the art can be used. The method for preparing three-dimensional graphene oxide preferably includes: preparing three-dimensional graphene oxide from a graphene oxide dispersion by a vacuum filtration-assisted template casting method; the concentration of the graphene oxide dispersion is 7 to 9 mg / L.

[0047] The present invention also provides the use of the three-dimensional graphene in preparing materials with metallic carrier characteristics.

[0048] The three-dimensional graphene prepared by the present invention has metallic carrier characteristics and can be used as in-situ metal interconnection lines in all-carbon electronic devices.

[0049] The present invention provides a method for in-situ triggering a metallic carrier transport mode in three-dimensional graphene oxide. The method constructs more wrinkled morphologies of a "percolation network" configuration on the surface of three-dimensional graphene through plastic stretching and reduction treatment, and the wrinkled morphology on the surface of three-dimensional graphene can realize a metallic carrier transport mode, that is, the energy band structure is transformed from a band gap open type to a band gap overlapping type. It is confirmed by the embodiments of the present invention that after the three-dimensional graphene oxide is treated by a method including liquid phase reduction and plastic stretching, the conductivity decreases with the increase of temperature, from 2.7 to 3.4 (100K) to 1.7 to 2.2 (300K).

[0050] The present invention provides a method for in-situ triggering of a metallic carrier transport mode in three-dimensional graphene oxide, which can avoid the inconvenience of executing traditional doping technologies such as element doping and field effect doping, and achieve regulation of local micro-regions and global carrier transport modes; in addition, the three-dimensional graphene containing a wrinkled morphology still retains the inherent mechanical properties advantages of graphene, such as light weight, high strength, flexibility, etc.

[0051] In order to further illustrate the present invention, the following examples are provided for detailed description. The raw materials used in the following examples of the present invention are all commercially available commodities.

[0052] Example 1

[0053] In this embodiment, a drawing device is used to prepare three-dimensional graphene. The drawing device consists of a drawing groove and four rollers. The rollers arranged along the direction of the drawn object are: driving roller 1 (drawing axis), transmission roller 1, transmission roller 2 and driving roller 2 (drawing axis). Figure 1 As shown, the drawing tank is filled with a liquid working medium (reducing agent solution), the transmission roller 1 and the transmission roller 2 are immersed in the liquid working medium, the driving roller 1 and the driving roller 2 are outside the drawing tank, the driving roller 1 and the driving roller 2 are the drawing axes, the linear speed of the driving roller 1 is V0, and the linear speed of the driving roller 2 is V1; V1-V0=0.25 rpm.

[0054] The method for preparing three-dimensional graphene in this embodiment comprises the following steps:

[0055] (1) A graphene oxide dispersion with a concentration of 7 mg / L (graphene oxide monolayer rate greater than 90%, characteristic size 12 μm (maximum in-plane straight line distance), and zeta potential 30 mV) was selected as the raw material. The graphene oxide dispersion was placed in a filtration device under a relative humidity of 60%, and three-dimensional graphene oxide was prepared by vacuum filtration-assisted template casting. The macroscopic shape of the three-dimensional graphene oxide was a thin film with a thickness of about 50 μm.

[0056] (2) The three-dimensional graphene oxide flakes obtained in step (1) are loaded into a driving roller device, and the connection position is fixed by double-sided tape, such as Figure 1 As shown, the three-dimensional graphene oxide between the driving roller 1 and the driving roller 2 is placed in the liquid working medium for 3 minutes.

[0057] (3) Mechanical load stretching process: Drive roller 1 and drive roller 2 are turned on synchronously, and the linear speed difference between the two is 0.25 rpm (the speed V0 of drive roller 1 is 1 rpm, and the speed V1 of drive roller 2 is 1.25 rpm). The single working time of the drive roller is 5 s, and the mechanical state is maintained for 10 s after the drive roller is completed.

[0058] (4) The three-dimensional graphene oxide after plasticization and stretching treatment is subjected to liquid phase reduction treatment: the three-dimensional graphene oxide is completely immersed in a mixed solution of anhydrous ethanol and hydrogen iodide for reduction treatment (the volume ratio of anhydrous ethanol and hydrogen iodide is 1:1), and the liquid phase reduction treatment lasts for 3 minutes.

[0059] (5) The three-dimensional graphene after the liquid phase reduction treatment is subjected to high-temperature heat treatment, the heat treatment temperature is 2500K, and the heat treatment time is 5 hours.

[0060] The microscopic morphology of three-dimensional graphene after plasticization and stretching treatment is as follows: Figure 2 As shown in Figure 2, the sample has a typical wrinkle microstructure. Figure 3 As shown, the conductivity of the sample shows a monotonically decreasing trend with increasing temperature, which has typical metallic carrier transport characteristics.

[0061] Example 2

[0062] This embodiment adopts the drafting device in Embodiment 1, and the preparation method of three-dimensional graphene includes the following steps:

[0063] (1) A graphene oxide dispersion with a concentration of 7 mg / L (graphene oxide monolayer rate greater than 90%, characteristic size 12 μm, and ZETA potential 30 mV) was selected as the raw material, and three-dimensional graphene oxide was prepared by vacuum filtration-assisted template casting under an environment with a relative humidity of 60%. The macroscopic shape of the three-dimensional graphene oxide was a thin film with a thickness of about 50 μm.

[0064] (2) The sheet-like three-dimensional graphene oxide prepared in step (1) is loaded into the driving roller device, and the connection position is fixed by double-sided tape. The three-dimensional graphene between the driving roller 1 and the driving roller 2 is placed in the liquid working medium for 3 minutes.

[0065] (3) Mechanical load stretching process: Drive roller 1 and drive roller 2 are turned on synchronously, and the linear speed difference between the two is 0.25 rpm (the speed of drive roller 1 is 0.25 rpm, and the speed of drive roller 2 is 0.5 rpm). The single working time of the drive roller is 5 s, and the mechanical state is maintained for 10 s after the drive roller is completed.

[0066] (4) The three-dimensional graphene oxide after the plasticization and stretching treatment is subjected to a liquid phase reduction treatment, and the three-dimensional graphene oxide is completely immersed in a mixed solution of anhydrous ethanol and hydrogen iodide for reduction treatment (volume ratio is 1:1), and the liquid phase reduction treatment lasts for 3 minutes.

[0067] (5) The three-dimensional graphene after the liquid phase reduction treatment is subjected to high-temperature heat treatment, the heat treatment temperature is 2500K, and the heat treatment time is 5 hours.

[0068] The microscopic morphology of three-dimensional graphene after plasticization and stretching treatment is as follows: Figure 4 As shown in Figure 2, the sample has a typical wrinkle microstructure. Figure 5 As shown, the conductivity of the sample shows a monotonically decreasing trend with increasing temperature, which has typical metallic carrier transport characteristics.

[0069] Example 3

[0070] This embodiment adopts the drafting device in Embodiment 1, and the preparation method of three-dimensional graphene includes the following steps:

[0071] (1) A graphene oxide dispersion with a concentration of 7 mg / L (graphene oxide monolayer rate greater than 90%, characteristic size 12 μm, and ZETA potential 30 mV) was selected as the raw material, and three-dimensional graphene oxide was prepared by vacuum filtration-assisted template casting under an environment with a relative humidity of 60%. The macroscopic shape of the three-dimensional graphene oxide was a thin film with a thickness of about 50 μm.

[0072] (2) The sheet-like three-dimensional graphene oxide obtained in step (1) is loaded into the driving roller device, and the connection position is fixed by double-sided tape. The three-dimensional graphene oxide between the driving roller 1 and the driving roller 2 is placed in the liquid working medium for 3 minutes.

[0073] (3) Mechanical load drafting process: Drive roller 1 and drive roller 2 are turned on synchronously, and the linear speed difference between the two is maintained at 0.25 rpm (the speed of drive roller 1 is 0.5 rpm, and the speed of drive roller 2 is 0.75 rpm). The single working time of the drive roller is 5 s, and the mechanical state is maintained for 10 s after the drive roller is completed.

[0074] (4) The three-dimensional graphene oxide after the plasticization and stretching treatment is subjected to a liquid phase reduction treatment, and the three-dimensional graphene oxide is completely immersed in a mixed solution of anhydrous ethanol and hydrogen iodide for reduction treatment (volume ratio is 1:1), and the liquid phase reduction treatment lasts for 3 minutes.

[0075] (5) The three-dimensional graphene after the liquid phase reduction treatment is subjected to high-temperature heat treatment, the heat treatment temperature is 2500K, and the heat treatment time is 5 hours.

[0076] The microscopic morphology of three-dimensional graphene after plasticization and stretching treatment is as follows: Figure 6 As shown in Figure 2, the sample has a typical wrinkle microstructure. Figure 7 As shown, the conductivity of the sample shows a monotonically decreasing trend with increasing temperature, which has typical metallic carrier transport characteristics.

[0077] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing three-dimensional graphene, It is characterized in that include: (1) performing a first reduction treatment on the flaky three-dimensional graphene oxide to obtain a first intermediate product; the first reduction treatment specifically comprises: mixing the flaky three-dimensional graphene oxide with a reducing agent solution; the reducing agent solution is a hydrogen iodide solution, and the hydrogen iodide solution is obtained by mixing ethanol and hydrogen iodide; (2) stretching the first intermediate product to obtain a second intermediate product; the stretching is performed in a reducing agent solution; the stretching is specifically: The first intermediate product is sequentially wrapped around and contacted with the drawing shaft; The rotation speed of the drafting shaft increases along the advancing direction of the second intermediate product; The number of drafting axes is ≥2; the linear speed difference between two adjacent drafting axes is 0.2~0.3 rpm; (3) performing a second reduction treatment on the second intermediate product to obtain three-dimensional graphene; the second reduction treatment specifically comprises: mixing the second intermediate product with a reducing agent solution; and performing a heat treatment on the second intermediate product after the second reduction treatment; The temperature of the heat treatment is 2500~3500 K.

2. The method for preparing three-dimensional graphene according to claim 1, It is characterized in that In step (1), the mixing time is 3 to 5 minutes; The stretching time is 15 to 30 s; In step (3), the mixing time is 3 to 5 minutes.

3. A drawing device for the method for preparing three-dimensional graphene according to claim 1, It is characterized in that include: A drawing tank for containing a reducing agent solution; the reducing agent solution is a hydrogen iodide solution obtained by mixing ethanol and hydrogen iodide; A drafting axis arranged along the advancing direction of the drafted object; The number of drafting axes is ≥2; The rotation speed of the drafting shaft increases along the forward direction of the drafted material; the linear speed difference between two adjacent drafting shafts is 0.2~0.3 rpm.

4. Use of the three-dimensional graphene prepared by the method for preparing three-dimensional graphene as claimed in any one of claims 1 to 2 in preparing materials with metallic carrier characteristics.

Citation Information

Patent Citations

  • Three-dimensional graphene with nano-micron graded pore structure and preparation method of three-dimensional graphene

    CN107032329A

  • Flexible graphene fibers and continuous preparation method thereof

    CN107151835A

  • Preparation method of flexible self-supporting three-dimensional porous graphene film

    CN108530073A

  • Structure and function integrated graphene material and preparation method thereof

    CN111003703A

  • Continuous preparation method and system of graphene film with directional heat conduction function