A metal ion pre-embedded vanadium oxide and its preparation and application
By pre-embedding metal ions in vanadium oxide, the problems of low conductivity and structural collapse of vanadium oxide materials are solved, the electrochemical performance and cycle stability of zinc ion batteries are improved, and more efficient energy density and power density are achieved. .
Patent Information
- Application Number
- CN202310256110.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-16
AI Technical Summary
The low conductivity of vanadium oxide materials in zinc-ion batteries and the capacity and cycle stability problems caused by crystal structure collapse during fast charging and discharging limit the performance and application of zinc-ion batteries.
By pre-embedding of metal ions (such as Na+, Zn2+, Al3+) in vanadium oxides, the layer spacing and electron conductivity are enhanced, the stability of the material and ion diffusion kinetics are improved, and the electrochemical performance is improved.
It significantly improves the electrochemical performance of vanadium oxide, extends the cycle life of the battery positive electrode material, and reduces the preparation cost, achieving more efficient energy and power density.
Smart Images

Figure CN116282158B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of zinc ion batteries, and in particular to a metal ion pre-embedded vanadium oxide and a preparation method and application thereof. Background Art
[0002] Since the 21st century, the energy consumption of countries around the world has been increasing day by day, the scale of energy exploitation has been expanding, and the large-scale use of traditional fossil resources, such as coal resources, oil resources, and natural gas resources, has caused serious environmental, energy, and climate problems. The sustainable development of the earth and mankind is facing severe challenges. Therefore, it is an inevitable trend and requirement of the development of the times to develop renewable energy, especially natural clean energy, to achieve sustainable long-term supply of energy consumption in human society. However, the existing renewable energy sources are intermittent energy sources. In order to ensure a continuous and reliable energy supply, energy storage systems of corresponding scale are required to store and transmit these energies. Since the 1990s, lithium-ion batteries have dominated the energy storage market. However, the development of lithium-ion batteries has also encountered troubles. Large-scale applications bring potential safety issues. Coupled with the shortage of lithium resources, the manufacturing cost of lithium batteries remains high. These problems have seriously restricted the large-scale energy storage application of lithium-ion batteries, and also caused great resistance to the sustainable development of renewable energy.
[0003] Zinc-ion batteries have low redox potential (-0.763 V vs. standard hydrogen electrode) and high theoretical capacity (820 mAh / g and 5855 mAh / cm 3 ), wide operating voltage window (0-2.0V), low cost, high safety, and environmental friendliness have attracted the attention of a large number of researchers in academia and industry worldwide. In addition, most zinc-ion batteries use aqueous solutions containing zinc salts as electrolytes, which are cheaper, safer, and more environmentally friendly. At the same time, the conductivity of aqueous electrolytes (up to 10 -1 -10S / cm) is much higher than the conductivity of organic electrolyte (10 -3 -10 -2 S / cm). During the operation of the battery, zinc ions are stripped / deposited from the metal zinc negative electrode, transported through the electrolyte, and then embedded / extracted from the positive electrode material. The positive electrode material is the main material that determines the energy density and power density of the battery. Therefore, the key to improving the performance of zinc-ion batteries is to optimize the positive electrode material.
[0004] To date, the materials that can be used for zinc ion embedding / extraction mainly include transition metal-based oxides with layered or channel structures, such as manganese-based oxides and vanadium-based oxides, as well as Prussian blue and its derivatives and organic compounds with open structures. Among the above materials, vanadium-based materials have shown great application potential due to their diverse morphologies and multivalent states, abundant raw material sources, low cost and high theoretical specific capacity. However, many layered vanadium oxides have low conductivity, and the crystal structure is prone to collapse under fast and deep charge and discharge conditions, which is bound to affect the reversible capacity and cycle stability of the material. In 2018, Liang Shuquan and others designed a V2O5 material as the positive electrode of an aqueous zinc ion battery. However, the volume expansion of the simple V2O5 material in the initial cycle will cause cracks and voids in the electrode, resulting in lower capacity and poor rate performance.
[0005] In response to the above problems, in recent years, researchers have tried to improve the electrochemical performance of vanadium-based materials through various means, including designing composite materials, using cation intercalation, etc. For example, the Chinese invention patent with application publication number 201910310607.2 discloses a vanadium oxide / clay composite positive electrode active material for aqueous batteries, positive electrode materials, and their preparation and application. The vanadium oxide / clay composite positive electrode active material is a two-dimensional V 10 O 24 ·12H2O. The test results show that the vanadium oxide / clay composite material in this example has a -1 At a current of 100 cycles, the specific capacity is 173 mAh g -1 , the capacity retention rate is about 95%. The preparation method of this invention is simple and easy, which can make the positive electrode material have good hydrophilicity and solve the problem of insufficient ion diffusion performance of positive electrode materials of aqueous batteries. However, the capacity of the battery after compounding with clay is not ideal, which is far lower than the theoretical capacity of vanadium-based materials. In addition, since the solid powder is directly stirred during the synthesis preparation, it will make the particles easy to aggregate and it is impossible to ensure that the particles are completely and evenly dispersed in the solution. Summary of the invention
[0006] In order to solve the above problems, the purpose of the present invention is to provide a metal ion pre-embedded vanadium oxide and its preparation and application. In order to improve the low conductivity and slow ion diffusion of vanadium-based materials, metal ions are pre-embedded in vanadium oxide to obtain metal ion pre-embedded vanadium oxide (abbreviated as M-NVO, M is selected from Na + 、Zn 2+ 、Al 3+One or more of these can expand the interlayer spacing of the main structure of the material, have a "pillar effect" that enhances the layered structure, and prevent destructive structural changes during ion insertion / extraction. While enhancing electronic conductivity after pre-embedding some metal ions, it improves the stability of the material, reduces the dissolution problem of vanadium oxide, and promotes diffusion kinetics, thereby significantly improving the electrochemical performance of the material.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] The first object of the present invention is to provide a method for preparing metal ion pre-embedded vanadium oxide, comprising the following steps:
[0009] (1) mixing a surfactant and water to obtain a surfactant solution;
[0010] (2) mixing the vanadium source and the surfactant solution prepared in step (1), and performing post-treatment to obtain a primary mixed solution;
[0011] (3) mixing the metal salt with the primary mixed solution prepared in step (2) to obtain a secondary mixed solution;
[0012] (4) transferring the secondary mixed solution obtained in step (3) to a polytetrafluoroethylene liner for hydrothermal reaction to obtain a mixed suspension;
[0013] (5) The mixed suspension obtained in step (4) is centrifuged, washed, and then post-treated to obtain metal ions pre-embedded in vanadium oxide.
[0014] In one embodiment of the present invention, in step (1), the surfactant is selected from F127 or One of P123;
[0015] The dosage ratio of surfactant to water is 468 mg:30 mL.
[0016] In one embodiment of the present invention, in step (1), the surfactant and water are mixed by heating and stirring in a water bath at a temperature of 60-80° C., a rotation speed of 1200-1500 r / min, and a time of 30-40 min.
[0017] In one embodiment of the present invention, in step (2), the vanadium source is selected from one or more of vanadium chloride, vanadium pentoxide, and ammonium metavanadate;
[0018] The mass ratio of the vanadium source to the surfactant is 1:1.
[0019] In one embodiment of the present invention, in step (2), the post-treatment is to adjust the pH of the solution to 2-3 using hydrochloric acid.
[0020] In one embodiment of the present invention, in step (3), the metal salt is selected from one or more of sodium chloride, zinc chloride or aluminum chloride;
[0021] The molar ratio of the metal salt to the vanadium source is 4:1-6.
[0022] In one embodiment of the present invention, in step (3), the mixing process is stirring, and the stirring time is 5-10 minutes.
[0023] In one embodiment of the present invention, in step (4), during the hydrothermal reaction, the temperature is 160-180° C. and the time is 10-24 h.
[0024] In one embodiment of the present invention, in step (5), during the centrifugal washing process, the washing solvent is a mixed solution of deionized water and ethanol; the post-treatment is a vacuum drying process, and during the vacuum drying process, the temperature is 60-80°C and the time is 8-12h.
[0025] The second object of the present invention is to provide a metal ion pre-intercalated vanadium oxide prepared by the above method.
[0026] The third object of the present invention is to provide an application of metal ion pre-embedded vanadium oxide in the preparation of a positive electrode material, wherein the positive electrode material is prepared by mixing metal ion pre-embedded vanadium oxide, a conductive agent and a binder in a mass ratio of 6-8:1-2:1-2 and then pressing the mixture onto a current collector using a tablet press.
[0027] The loading of metal ions pre-embedded into vanadium oxide in the cathode material is 1.5-2.0 mg cm -2 .
[0028] In one embodiment of the present invention, the conductive agent is one or more of Ketjen black, acetylene black, Super-P or graphite conductive agent;
[0029] The binder is one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol or sodium carboxymethyl cellulose.
[0030] The current collector is a titanium mesh, a chromium mesh or a carbon cloth.
[0031] Furthermore, the above-mentioned positive electrode material is combined with a negative electrode material, an aqueous electrolyte and a separator to obtain an aqueous battery;
[0032] Wherein, the aqueous electrolyte is selected from one or both of zinc trifluoromethanesulfonate and zinc sulfate aqueous solution;
[0033] The negative electrode material is a zinc foil with a thickness of 90-100 μm;
[0034] The separator is selected from one of glass fiber and cellulose fiber membrane.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) Compared with the traditional preparation method, the vanadium-based compound particles prepared by the present invention are more uniform. By adding a surfactant during the synthesis process, the surface tension of the target solution is effectively reduced, which is beneficial to the dispersion of the main metal ions and prevents the aggregation of particles;
[0037] (2) The present invention innovatively regulates the growth environment of vanadium-based compounds by pH, thereby improving the crystallinity of the material while regulating the microscopic morphology of the material.
[0038] (3) Compared with the traditional synthesis method, the present invention adopts the method of metal ion pre-embedding, and selects different metal ions as guest ions to be pre-embedded in the vanadium oxide compound. The embedded ions act as a supporting "pillar" in the interlayer spacing of the vanadium oxide, which can prevent the collapse of the crystal structure of the vanadium-based material, widen the interlayer spacing of the vanadium oxide, and provide more active sites for ion embedding, which is beneficial to the improvement of battery capacity and the extension of the service life of the battery positive electrode material.
[0039] (4) The raw materials used in the present invention are abundant in reserves, low in preparation cost, short in cycle, and low in energy consumption. Applying them in the field of electrochemical energy storage devices has broad development prospects and considerable economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 XRD pattern of sodium ion pre-embedded vanadium oxide: Na-NVO prepared in Example 1;
[0041] Figure 2 This is a SEM image of the sodium ion pre-embedded vanadium oxide: Na-NVO prepared in Example 1;
[0042] Figure 3 The cyclic voltammetry curve of the sodium ion pre-intercalated vanadium oxide: Na-NVO prepared in Example 1;
[0043] Figure 4 XRD pattern of zinc ion pre-embedded vanadium oxide: Zn-NVO prepared in Example 2;
[0044] Figure 5 This is a SEM image of the zinc ion pre-embedded vanadium oxide: Zn-NVO prepared in Example 2;
[0045] Figure 6 This is a cyclic voltammetry curve of the zinc ion pre-embedded vanadium oxide: Zn-NVO prepared in Example 2;
[0046] Figure 7 XRD pattern of aluminum ion pre-embedded vanadium oxide: Al-NVO prepared in Example 3;
[0047] Figure 8 This is a SEM image of aluminum ion pre-embedded vanadium oxide: Al-NVO prepared in Example 3;
[0048] Fig. 9 The cyclic voltammetry curve of the aluminum ion pre-embedded vanadium oxide: Al-NVO prepared in Example 3;
[0049] Fig.10 The cyclic stability test diagrams are of Na-NVO prepared in Example 1, Zn-NVO prepared in Example 2, Al-NVO prepared in Example 3, and NVO prepared in Comparative Example 1. DETAILED DESCRIPTION
[0050] The present invention provides a method for preparing metal ion pre-embedded vanadium oxide, comprising the following steps:
[0051] (1) mixing a surfactant and water to obtain a surfactant solution;
[0052] (2) mixing the vanadium source and the surfactant solution prepared in step (1), and performing post-treatment to obtain a primary mixed solution;
[0053] (3) mixing the metal salt with the primary mixed solution prepared in step (2) to obtain a secondary mixed solution;
[0054] (4) transferring the secondary mixed solution obtained in step (3) to a polytetrafluoroethylene liner for hydrothermal reaction to obtain a mixed suspension;
[0055] (5) The mixed suspension obtained in step (4) is centrifuged, washed, and then post-treated to obtain metal ions pre-embedded in vanadium oxide.
[0056] In one embodiment of the present invention, in step (1), the surfactant is selected from F127 or One of P123;
[0057] The dosage ratio of surfactant to water is 468 mg:30 mL.
[0058] In one embodiment of the present invention, in step (1), the surfactant and water are mixed by heating and stirring in a water bath at a temperature of 60-80° C., a rotation speed of 1200-1500 r / min, and a time of 30-40 min.
[0059] In one embodiment of the present invention, in step (2), the vanadium source is selected from one or more of vanadium chloride, vanadium pentoxide, and ammonium metavanadate;
[0060] The mass ratio of the vanadium source to the surfactant is 1:1.
[0061] In one embodiment of the present invention, in step (2), the post-treatment is to adjust the pH of the solution to 2-3 using hydrochloric acid.
[0062] In one embodiment of the present invention, in step (3), the metal salt is selected from one or more of sodium chloride, zinc chloride or aluminum chloride;
[0063] The molar ratio of the metal salt to the vanadium source is 4:1-6.
[0064] In one embodiment of the present invention, in step (3), the mixing process is stirring, and the stirring time is 5-10 minutes.
[0065] In one embodiment of the present invention, in step (4), during the hydrothermal reaction, the temperature is 160-180° C. and the time is 10-24 h.
[0066] In one embodiment of the present invention, in step (5), during the centrifugal washing process, the washing solvent is a mixed solution of deionized water and ethanol; the post-treatment is a vacuum drying process, and during the vacuum drying process, the temperature is 60-80°C and the time is 8-12h.
[0067] The invention provides a metal ion pre-embedded vanadium oxide prepared by the method.
[0068] The present invention provides an application of metal ion pre-embedded vanadium oxide in the preparation of positive electrode materials. The positive electrode material is prepared by mixing metal ion pre-embedded vanadium oxide, a conductive agent and a binder in a mass ratio of 6-8:1-2:1-2 and then pressing the mixture onto a current collector using a tablet press.
[0069] The loading of metal ions pre-embedded into vanadium oxide in the cathode material is 1.5-2.0 mg cm -2 .
[0070] In one embodiment of the present invention, the conductive agent is one or more of Ketjen black, acetylene black, Super-P or graphite conductive agent;
[0071] The binder is one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol or sodium carboxymethyl cellulose.
[0072] The current collector is a titanium mesh, a chromium mesh or a carbon cloth.
[0073] Furthermore, the above-mentioned positive electrode material is combined with a negative electrode material, an aqueous electrolyte and a separator to obtain an aqueous battery;
[0074] Wherein, the aqueous electrolyte is selected from one or both of zinc trifluoromethanesulfonate and zinc sulfate aqueous solution;
[0075] The negative electrode material is a zinc foil with a thickness of 90-100 μm;
[0076] The separator is selected from one of glass fiber and cellulose fiber membrane.
[0077] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0078] In the following examples, unless otherwise specified, all reagents used are commercially available reagents with analytical purity, and all detection means and methods used are conventional detection means and methods in the art.
[0079] In the following embodiments, the concentration of hydrochloric acid is 3M, and the zinc sheet is a zinc foil with a thickness of 95 μm (the thickness may also be 90-100 μm).
[0080] Example 1
[0081] This embodiment provides a sodium ion pre-embedded vanadium oxide and its preparation and application.
[0082] (1) 468 mg F127 solid was added into 30 ml of deionized water, heated in a water bath at 60°C, and stirred at 1500 r / min for 30 min to obtain F127 solution;
[0083] (2) Add 468 mg of ammonium metavanadate solid powder to the mixture obtained in step (1) F127 solution, mix well to obtain a light yellow clear solution, then let the light yellow clear solution stand to room temperature, adjust the pH to 2.0 with hydrochloric acid, and it will become an orange clear solution: a mixed solution;
[0084] (3) adding 350.64 mg of sodium chloride solid powder to the primary mixed solution obtained in step (2), stirring at room temperature for 10 min at a speed of 800 r / min to obtain a secondary mixed solution;
[0085] (4) transferring the secondary mixed solution obtained in step (3) into a 50 ml polytetrafluoroethylene liner, and then placing it in a forced air drying oven at 180° C. for 24 hours to perform a hydrothermal reaction to obtain a mixed suspension;
[0086] (5) The mixed suspension obtained in step (4) was centrifuged and washed with deionized water and ethanol (centrifuged and washed 3 times), and then placed in a vacuum drying oven at 80° C. for 8 h to obtain sodium ion pre-embedded vanadium oxide, namely Na-NVO (XRD pattern as shown in FIG. Figure 1 As shown in the SEM images Figure 2 The cyclic voltammetry curve is shown in Figure 3 shown).
[0087] The sodium ion pre-embedded vanadium oxide, Ketjen black and PTFE prepared above were mixed and ground evenly in a mass ratio of 7:2:1, dissolved in ethanol to prepare a film with a thickness of 10-50 μm, and then pressed onto a titanium mesh with a diameter of 10 mm using a tablet press. After drying, a sodium ion pre-embedded vanadium oxide electrode was obtained.
[0088] The sodium ion pre-embedded vanadium oxide electrode prepared above was used as the positive electrode, the glass fiber was used as the separator, the negative electrode was a zinc sheet with a diameter of 10 mm, and the electrolyte was 150 μL of a 2.5 M aqueous solution of zinc trifluoromethanesulfonate. An aqueous zinc ion button cell was assembled (the cycle stability test diagram is shown in FIG. Fig.10 shown).
[0089] Example 2
[0090] This embodiment provides a zinc ion pre-embedded vanadium oxide and its preparation and application.
[0091] (1) 468 mg P123 solid was added into 30 ml of deionized water, heated in a water bath at 70°C, and stirred at 1300 r / min for 35 min to obtain P123 solution;
[0092] (2) Add 468 mg of ammonium metavanadate solid powder to the mixture obtained in step (1) P123 solution, mix well to obtain a light yellow clear solution, then let the light yellow clear solution stand to room temperature, adjust the pH to 2.5 with hydrochloric acid, and it will become an orange clear solution: a mixed solution;
[0093] (3) adding 817.89 mg of zinc chloride solid powder to the primary mixed solution obtained in step (2), stirring at room temperature for 5 min at a speed of 800 r / min to obtain a secondary mixed solution;
[0094] (4) transferring the secondary mixed solution obtained in step (3) into a 50 ml polytetrafluoroethylene liner, and then placing it in a forced air drying oven at 170° C. for 15 hours to perform a hydrothermal reaction to obtain a mixed suspension;
[0095] (5) The mixed suspension obtained in step (4) was centrifuged and washed with deionized water and ethanol (centrifuged and washed 3 times), and then placed in a vacuum drying oven and dried at 70° C. for 12 h to obtain zinc ion pre-embedded vanadium oxide, namely Zn-NVO (XRD pattern as shown in FIG. Figure 4 As shown in the SEM images Figure 5 The cyclic voltammetry curve is shown in Figure 6 shown).
[0096] The zinc ion pre-embedded vanadium oxide, acetylene black and PVDF prepared above were mixed and ground evenly in a mass ratio of 8:1:1, dissolved in ethanol to prepare a film with a thickness of 10-50 μm, and then pressed onto a titanium mesh with a diameter of 10 mm using a tablet press. After drying, a zinc ion pre-embedded vanadium oxide electrode was obtained.
[0097] The prepared zinc ion pre-embedded vanadium oxide electrode was used as the positive electrode, the glass fiber was used as the separator, the negative electrode was a zinc sheet with a diameter of 10 mm, and the electrolyte was 150 μL of a 2.5 M aqueous solution of zinc trifluoromethanesulfonate. An aqueous zinc ion button cell was assembled (the cycle stability test diagram is shown in FIG. Fig.10 shown).
[0098] Example 3
[0099] This embodiment provides an aluminum ion pre-embedded vanadium oxide and its preparation and application.
[0100] (1) 468 mg F127 solid was added into 30 ml of deionized water, heated in a water bath at 80°C, and stirred at 1200 r / min for 40 min to obtain F127 solution;
[0101] (2) Add 468 mg of ammonium metavanadate solid powder to the mixture obtained in step (1) F127 solution, mix well to obtain a light yellow clear solution, then let the light yellow clear solution stand to room temperature, adjust the pH to 3.0 with hydrochloric acid, and it will become an orange clear solution: a mixed solution;
[0102] (3) adding 800 mg of aluminum chloride solid powder to the primary mixed solution obtained in step (2), stirring at room temperature for 8 min at a speed of 800 r / min to obtain a secondary mixed solution;
[0103] (4) transferring the secondary mixed solution obtained in step (3) into a 50 ml polytetrafluoroethylene liner, and then placing it in a forced air drying oven at 160° C. for 10 hours to perform a hydrothermal reaction to obtain a mixed suspension;
[0104] (5) The mixed suspension obtained in step (4) was centrifuged and washed with deionized water and ethanol (centrifuged and washed 3 times), and then placed in a vacuum drying oven at 60° C. for 10 h to obtain aluminum ion pre-embedded vanadium oxide, namely Al-NVO (XRD pattern as shown in FIG. Figure 7 As shown in the SEM images Figure 8 The cyclic voltammetry curve is shown in Fig. 9 shown).
[0105] The aluminum ion pre-embedded vanadium oxide, Super-P and PTFE prepared above were mixed and ground evenly in a mass ratio of 6:2:2, dissolved in ethanol to prepare a film with a thickness of 10-50 μm, and then pressed onto a titanium mesh with a diameter of 10 mm using a tablet press. After drying, an aluminum ion pre-embedded vanadium oxide electrode was obtained.
[0106] The aluminum ion pre-embedded vanadium oxide electrode prepared above was used as the positive electrode, the glass fiber was used as the separator, the negative electrode was a zinc sheet with a diameter of 10 mm, and the electrolyte was 150 μL of a 2.5 M aqueous solution of zinc trifluoromethanesulfonate. An aqueous zinc ion button cell was assembled (the cycle stability test diagram is shown in FIG. Fig.10 shown).
[0107] Comparative Example 1
[0108] Compared with Example 1, this comparative example is the same as Example 1 except that sodium chloride solid powder is not added, and vanadium oxide without pre-embedded metal ions, called NVO, is prepared.
[0109] The prepared vanadium oxide without pre-embedded metal ions, Super-P and PTFE were mixed and ground evenly in a mass ratio of 6:2:2, dissolved in ethanol to prepare a film with a thickness of 10-50 μm, and then pressed onto a titanium mesh with a diameter of 10 mm using a tablet press. After drying, a vanadium oxide electrode without pre-embedded metal ions was obtained.
[0110] The above-prepared vanadium oxide electrode without pre-embedded metal ions was used as the positive electrode, the glass fiber was used as the separator, the negative electrode was a zinc sheet with a diameter of 10 mm, and the electrolyte was 150 μL of a 2.5 M aqueous solution of zinc trifluoromethanesulfonate. An aqueous zinc ion button cell was assembled (the cycle stability test diagram is shown in FIG. Fig.10 shown).
[0111] The metal ion pre-embedded vanadium oxide materials prepared in the above embodiments were subjected to SEM test and XRD test. Figure 1 , Figure 4 and Figure 7 As shown in the figure, the XRD patterns show that the three synthesized materials have good crystallinity and can correspond to the physical phases in the standard card (the sample diffraction pattern and the PDF card library after the given search conditions), indicating that Na 0.33V2O5, NH4V3O8 and Zn3(OH)2V2O7 dual phase and H 11 Al2V6O 23.2 Materials. From the SEM images, we can see that Na-NVO( Figure 2 ) showed a flat, ribbon-like morphology with a very uniform size, about 30 μm in length and 100-150 nm in width; Zn-NVO( Figure 5 ) is a mixture of needle-shaped and rod-shaped; Al-NVO( Figure 8 ) appears as a cluster of larger particles.
[0112] The aqueous zinc ion button cells assembled in the above embodiments were subjected to cyclic voltammetry tests. The cyclic voltammetry curves are shown in FIG. Figure 3 , Figure 6 and Fig. 9 As shown, all CV curves have two pairs of redox peaks, V 5+ / V 4+ and V 4+ / V 3+ The redox peaks of Zn are located at 1.0 / 0.93 and 0.63 / 0.52 V, respectively. 2+ The extraction / insertion of is a multi-step behavior during the charge-discharge process. The first cycle of CV is the activation process, and the next two cycles show almost overlapping curves, indicating that the synthesized material has good stability.
[0113] The aqueous zinc ion button cells assembled in the above embodiments were subjected to a cycle stability test. The test results are as follows: Fig.10 As shown, at a current density of 0.5A / g, the average discharge capacity of Na-NVO is about 300mAh / g, and the capacity retention rate is 74.68% after 50 charge and discharge cycles; the average discharge capacity of Zn-NVO is about 250mAh / g, and the capacity retention rate is 92.75% after 50 charge and discharge cycles; the average discharge capacity of Al-NVO is about 200mAh / g, and the capacity retention rate is 86.45% after 50 charge and discharge cycles; the average discharge capacity of NVO is about 220mAh / g, and the capacity retention rate is only 47.54% after 50 charge and discharge cycles.
[0114] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing metal ion pre-embedded vanadium oxide, characterized in that: The following steps are involved: (1) mixing the surfactant and water by heating in a water bath and stirring to obtain a surfactant solution; Wherein, the surfactant is selected from one of Pluronic® F127 or Pluronic® P123; (2) mixing the vanadium source and the surfactant solution prepared in step (1), and adjusting the pH of the solution to 2-3 using hydrochloric acid to obtain a primary mixed solution; (3) mixing the metal salt with the primary mixed solution prepared in step (2) to obtain a secondary mixed solution; (4) subjecting the secondary mixed solution obtained in step (3) to a hydrothermal reaction to obtain a mixed suspension; Wherein, during the hydrothermal reaction, the temperature is 160-180°C; (5) The mixed suspension obtained in step (4) is centrifuged, washed, and then post-treated to obtain metal ions pre-embedded into vanadium oxide.
2. The method for preparing metal ion pre-embedded vanadium oxide according to claim 1, characterized in that: In step (1), the ratio of surfactant to water is 468 mg:30 mL.
3. The method for preparing metal ion pre-embedded vanadium oxide according to claim 1, characterized in that: In step (1), during the water bath heating and stirring process, the temperature is 60-80°C, the rotation speed is 1200-1500 r / min, and the time is 30-40 min.
4. The method for preparing metal ion pre-embedded vanadium oxide according to claim 1, characterized in that: In step (2), the vanadium source is selected from one or more of vanadium chloride, vanadium pentoxide, and ammonium metavanadate; The mass ratio of the vanadium source to the surfactant is 1:
1.
5. The method for preparing metal ion pre-embedded vanadium oxide according to claim 1, characterized in that: In step (3), the metal salt is selected from one or more of sodium chloride, zinc chloride or aluminum chloride; The molar ratio of the metal salt to the vanadium source is 4:1-6.
6. The method for preparing metal ion pre-embedded vanadium oxide according to claim 1, characterized in that: In step (4), the hydrothermal reaction time is 10-24 hours.
7. The method for preparing metal ion pre-embedded vanadium oxide according to claim 1, characterized in that: In step (5), during the centrifugal washing process, the washing solvent is a mixed solution of deionized water and ethanol; the post-treatment is a vacuum drying process, and during the vacuum drying process, the temperature is 60-80°C and the time is 8-12 hours.
8. A metal ion pre-embedded vanadium oxide prepared by the method according to any one of claims 1 to 7.
9. A use of the metal ion pre-embedded vanadium oxide as claimed in claim 8 in the preparation of a positive electrode material, characterized in that: The positive electrode material is prepared by mixing metal ions pre-embedded in vanadium oxide, a conductive agent and a binder in a mass ratio of 6-8:1-2:1-2 and then pressing the mixture onto a current collector using a tablet press. The loading of metal ions pre-embedded into vanadium oxide in the cathode material is 1.5-2.0 mg cm -2 .