Anti-glare glass and preparation method thereof, and display device
By adjusting the raw material ratio and thermal processing, the problem of low gloss of traditional anti-glare glass is solved, and high-gloss anti-glare glass is prepared for use in display devices, which improves the visual effect and touch experience.
Patent Information
- Application Number
- CN202310115571.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-15
AI Technical Summary
Traditional anti-glare glass has low gloss and cannot meet the high gloss requirements of vehicle-mounted display devices, affecting the visual effect and touch experience.
Basic glass is prepared by adjusting the ratio of raw materials, and is combined with chemical etching, frosting and chemical polishing to form a roughened surface. The roughened surface is made smoother and glossier through thermal processing.
An anti-glare glass with a gloss higher than 114% is prepared to meet the high gloss requirements while maintaining the anti-glare effect and improving the visual effect and touch experience of the display device.
Smart Images

Figure CN116282903B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of glass technology, and in particular to an anti-glare glass and a preparation method thereof, and a display device. Background Art
[0002] With the development of smart cars, higher requirements are placed on the operability, precision and clarity of vehicle-mounted display devices. In order to ensure driving comfort and safety, while displaying clear information, the display device must also meet the anti-glare requirements. Anti-glare glass is made by chemical etching and other methods to roughen the glass surface, thereby reducing the mirror reflection of the glass and achieving the purpose of anti-glare. Although traditional anti-glare glass can reduce mirror reflection, the diffuse light it produces diffuses in all directions, resulting in a decrease in the gloss of the glass, affecting the visual effect of the display device. According to market feedback, the 60° glossiness of the vehicle-mounted display device is required to reach 110% to 130%, while the 60° glossiness of traditional anti-glare glass usually does not exceed 110%.
[0003] Therefore, how to prepare an anti-glare glass with higher gloss has become a technical problem that needs to be solved urgently. Summary of the invention
[0004] Based on this, the present application provides an anti-glare glass with high gloss and a preparation method thereof. In addition, the present application provides a display device including the anti-glare glass.
[0005] In a first aspect, the present application provides a method for preparing an anti-glare glass, comprising the following steps:
[0006] Melt and shape the raw materials to prepare basic glass;
[0007] Roughening a surface of a base glass to prepare a roughened glass;
[0008] The roughened glass is subjected to heat treatment to make the roughened surface smooth, thereby preparing the anti-glare glass;
[0009] Among them, according to mass percentage, the raw materials include the following components:
[0010]
[0011] And K 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages of ZrO is 0.2% to 5%. 2 The sum of the mass percentages of BaO and ZnO is 0.2% to 5%.
[0012] The method for preparing the anti-glare glass is as follows: first, a base glass with high gloss, chemical temperature and thermal stability is prepared by adjusting the ratio of raw materials; then, particles are precipitated on the surface of the base glass by roughening treatment to form a roughened surface with anti-glare effect, which effectively reduces mirror reflection; and then, the roughened glass is softened by thermal processing to increase the surface tension of the roughened surface, thereby increasing the size of the particles and making the roughened surface smoother, so that the diffuse reflected light generated by the surface of the anti-glare glass is more orderly and the glossiness is increased. Thus, the anti-glare glass prepared has a high glossiness while achieving the anti-glare effect, and the surface is relatively flat and smooth. When used to prepare a display device, it can improve the visual effect and touch experience of the display device.
[0013] In some embodiments, Al 2 O 3 The mass percentage is 16.8% to 21%;
[0014] and / or Na 2 The mass percentage of O is 12% to 14.8%;
[0015] and / or, the mass percentage of MgO is 2.9% to 5%;
[0016] and / or, K 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages is 3.2% to 5%;
[0017] and / or ZrO 2 The sum of the mass percentages of BaO and ZnO is 0.2% to 3.2%.
[0018] In some embodiments, the roughening process includes a chemical etching process, a sanding process, and a chemical polishing process performed sequentially.
[0019] In some embodiments, the thermal processing includes: performing a pressing process while heating the roughened glass.
[0020] In some embodiments, the pressing process comprises the following steps:
[0021] Pressed parts with smooth surfaces are respectively arranged on two surfaces of the roughened glass, and the smooth surfaces are in contact with the roughened glass.
[0022] In some embodiments, the preset temperature of the thermal processing is 580°C to 680°C;
[0023] And / or, the heat treatment holding time is 20min to 50min;
[0024] And / or, the heating rate of the thermal treatment is 8°C / min to 15°C / min.
[0025] In some embodiments, the temperature of the thermal processing is 590°C to 660°C.
[0026] In some of the embodiments, the preparation method further includes: before the roughening treatment, setting a protective film on one surface of the base glass, and then roughening the surface of the base glass facing away from the protective film; and after the roughening treatment and before the heat treatment, removing the protective film, and then heat treating the roughened glass.
[0027] In a second aspect, the present application provides an anti-glare glass, which is manufactured according to the method for manufacturing the anti-glare glass of the first aspect, and the 60° glossiness of the anti-glare glass is greater than or equal to 114%.
[0028] In a third aspect, the present application provides a display device comprising the anti-glare glass of the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A polarizing microscope image of a roughened surface of a base glass after roughening treatment according to an embodiment of the present application;
[0030] Figure 2 for Figure 1 A partial enlarged view of
[0031] Figure 3 for Figure 1 Polarized microscope image of the roughened surface of the base glass after thermal processing;
[0032] Figure 4 for Figure 3 A partial enlarged view of . DETAILED DESCRIPTION
[0033] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0034] In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically limited. "At least one" used in this application refers to any one, any two, or any two or more of the listed items. "Above a certain number" used in this application should be understood as a certain number and a range greater than a certain number.
[0035] The terms "and / or", "or / and", and "and / or" used in this application have an optional scope including any one of two or more related listed items, and also include any and all combinations of the related listed items, said any and all combinations including any combination of any two related listed items, any more related listed items, or all related listed items.
[0036] When “including”, “having” and “comprising” are used in the present application, it is intended to cover a non-exclusive inclusion, and another component may be added unless an explicit limiting term such as “only”, “consisting of”, etc. is used. Unless mentioned otherwise, a term in the singular form may include a plural form and shall not be construed as being one in number.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0038] Glossiness in this application refers to the percentage of the amount of reflected light on the surface of the sample to be tested to the amount of reflected light on the surface of the standard sample under the same conditions. Glossiness 60° refers to the glossiness test result obtained when the incident light is incident at an angle of 60 degrees to the surface normal of the sample to be tested and the standard sample. Glossiness 60° can be tested using a commercially available glossiness measuring instrument.
[0039] Traditional technology uses anti-glare treatment (or roughening treatment) to roughen the surface of the glass to achieve the anti-glare function. Understandably, when light is incident on the rough surface of the glass, diffuse reflection occurs, and the reflected light generated is irregularly reflected in different directions, effectively reducing the mirror reflection, and preventing strong reflected light from irritating the human eye, thereby achieving the purpose of anti-glare. However, when the roughness of the glass surface is too large, the displayed image will become blurred. The preparation process of traditional anti-glare glass mainly includes frosting and chemical polishing. The frosting treatment is used to roughen the glass surface to form a roughened surface with an anti-glare effect; the chemical polishing treatment is used to improve the roughness of the roughened surface and enhance the clarity and glossiness. However, after the chemical polishing treatment, the roughened surface of the glass is still relatively rough, so the diffuse reflected light generated on its surface is still relatively disordered, resulting in a low glossiness of the glass, affecting the user's visual experience.
[0040] The present application has found that the reason why the traditional anti-glare glass has a low glossiness is mainly because the chemical polishing treatment cannot effectively improve the roughness of the roughened surface. Specifically, the roughened surface of the anti-glare glass is usually composed of uneven textures, and the raised parts have a granular morphology. Since the curvatures of the particle surfaces are different at different places, when the light is incident on the surface of the particles, the normal directions of each place are inconsistent, causing the reflected light to be reflected in different directions. The traditional chemical polishing treatment uses the etching effect of the polishing liquid to make the particles smoother and rounder as a whole. The particle surfaces still have different curvatures at different places. Therefore, the traditional chemical polishing treatment has limited effect on the improvement of the glass glossiness. The present application improves the preparation process of anti-glare glass to make the surface of the particles smoother, thereby making the roughened surface of the glass smoother, and generating more orderly diffuse reflected light, thereby achieving the purpose of increasing the glossiness. In addition, by adjusting the raw material ratio, the glossiness of the anti-glare glass itself is increased, and its overall glossiness is further improved.
[0041] One embodiment of the present application provides a method for preparing an anti-glare glass, comprising steps S100 to S300.
[0042] Step S100: melting and molding the raw materials to prepare basic glass.
[0043] In some embodiments, the raw material includes the following components by weight:
[0044]
[0045] And K 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages of ZrO is 0.2% to 5%. 2 The sum of the mass percentages of BaO and ZnO is 0.2% to 5%.
[0046] By adjusting the ratio of raw materials, the obtained basic glass has higher chemical stability, thermal stability and glossiness. 2 、Al 2 O 3 、Na 2 O and MgO are the main components of the basic glass. By adjusting the content of these components, the chemical stability and thermal stability of the basic glass can be guaranteed; K 2 O. Li 2 O.B 2 O 3 、ZrO 2 , BaO and ZnO are used as components to improve the optical properties of glass, and K 2 O. Li 2 O and B 2 O3 At least one of the above three components can enhance the refractive index of the base glass, thereby increasing its own glossiness, and adjusting the total amount of the above three components can prevent the occurrence of crystallization; adding ZrO 2 , BaO and ZnO, and regulating their total addition amount can reduce the crystallization tendency of the glass and further improve the stability of the basic glass.
[0047] Silicon dioxide (SiO 2 ) is the main component of the glass skeleton, which can improve the thermal stability, chemical stability and ultraviolet light transmittance of the glass. 2 When the content of SiO2 (in terms of mass percentage of the total mass of the raw materials, unless otherwise specified, all contents mentioned below are mass percentages) is greater than 65%, a higher melting temperature is required when preparing the substrate glass, which causes crystallization of the base glass, affects its glossiness, and reduces the corrosion resistance of the base glass to chemical etching solutions; when SiO2 2 When the content of SiO is less than 55%, the forming performance of the base glass is poor, and the mechanical strength and optical properties do not meet the requirements. 2 The content of SiO is 55% to 65%, specifically 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64% or 65%. It can be understood that SiO 2 The content of may also be selected in the range of 55% to 65%.
[0048] Alumina (Al 2 O 3 ) is the main component of glass intermediates, which can improve the thermal stability, corrosion resistance to etching liquid, mechanical strength, hardness and refractive index of the base glass. 2 O 3 When the content of Al is less than 12%, the above properties of the base glass are poor; 2 O 3 When the content of Al is greater than 21%, the viscosity of the glass liquid will increase, making it more difficult to clarify the base glass. 2 O 3 The content of Al is 12% to 21%, specifically 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% or 21%. It can be understood that Al 2 O 3 The content of may also be selected in the range of 12% to 21%.
[0049] In some embodiments, Al 2 O 3 The mass percentage of Al is 16.8% to 21%,2 O 3 When the content is within the above range, the glossiness of the base glass can be further improved.
[0050] Sodium oxide (Na 2 O) acts as a flux to improve the melting properties of glass raw materials. 2 The content of O can improve the melting performance of the raw material, but when Na 2 When the O content is greater than 16%, the corrosion resistance and thermal stability of the glass will be reduced. 2 The content of O is 12% to 16%, specifically 12%, 13%, 14%, 15% or 16%. It is understandable that Na 2 The content of O may also be appropriately selected within the range of 12% to 16%.
[0051] In some embodiments, Na 2 The mass percentage of O is 12% to 14.8%, and the mass percentage of Na 2 When the content of O is within the above range, the meltability of the glass raw material can be further improved, and the glossiness of the base glass can be increased.
[0052] Magnesium oxide (MgO) can reduce the viscosity of glass liquid at high temperature, promote the melting of glass raw materials and the clarification of glass liquid, and improve the corrosion resistance of basic glass. When the content of MgO is less than 2%, the viscosity of glass liquid is relatively large and the melting performance of glass raw materials is relatively poor; when the content of MgO is greater than 5%, the glass is easy to drag. Based on this, the content of MgO is 2% to 5%, specifically 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%. It can be understood that the content of MgO can also be other suitable selections within the range of 2% to 5%.
[0053] In some embodiments, the mass percentage of MgO is 2.9% to 5% by mass. When the content of MgO is within the above range, the viscosity of the glass liquid can be further improved and the glossiness of the base glass can be increased.
[0054] Potassium oxide (K 2 O), lithium oxide (Li 2 O) and boron oxide (B 2 O 3 ) plays a role in fluxing. As an external oxide in the glass network, it can improve the melting performance of glass raw materials, reduce the viscosity of glass liquid, and reduce the tendency of glass crystallization. Adding K to the raw material formula 2 O. Li 2 O and B 2 O 3At least one of the above can effectively reduce the crystals precipitated in the base glass and increase the refractive index, transparency and glossiness of the base glass. 2 The mass percentage of O is 0-3%, Li 2 The mass percentage of O is 0-3%, B 2 O 3 The mass percentage of K is 0 to 3%. 2 The mass percentage of O is 0, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%, and the mass percentage of Li 2 The mass percentage of O is 0, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%, B 2 O 3 The mass percentage of K is 0, 0.5%, 1%, 1.5%, 2%, 2.5% or 3%. 2 O. Li 2 O and B 2 O 3 The mass percentage of K can also be independently selected in the range of 0 to 3%. 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages of K is 0.2% to 5%, specifically 0.2%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages may also be appropriately selected within the range of 0.2% to 5%.
[0055] In some embodiments, K 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages of K is 3.2% to 5%, 2 O. Li 2 O and B 2 O 3 When the sum of the mass percentages of is within the above range, the melting performance of the glass liquid can be further improved and the glossiness of the base glass can be increased.
[0056] Zirconia (ZrO 2 ), barium oxide (BaO) and zinc oxide (ZnO) are introduced as external oxides of the glass network to increase the gloss, chemical stability and thermal stability of the base glass. 2 At least one of ZrO, BaO and BaO can improve the above properties of the base glass.2 The mass percentage of ZrO is 0-2.3%, the mass percentage of BaO is 0-1.5%, and the mass percentage of ZnO is 0-2%. 2 The mass percentage of ZrO is 0, 0.4%, 0.8%, 1.2%, 1.5%, 2% or 2.3%, the mass percentage of BaO is 0, 0.4%, 0.8%, 1.2% or 1.5%, and the mass percentage of ZnO is 0, 0.4%, 0.8%, 1.2%, 1.6% or 2%. 2 Other suitable choices can be made in the range of 0-2.3%, the mass percentage of BaO can be made in the range of 0-1.5%, and the mass percentage of ZnO can be made in the range of 0-2%. 2 The sum of the mass percentages of BaO and ZnO is 0.2% to 5%, specifically 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, ZrO 2 The sum of the mass percentages of BaO and ZnO can also be appropriately selected within the range of 0.2% to 5%. When the sum of the mass percentages of the three exceeds 5%, crystallization is likely to occur, and the glossiness of the base glass cannot be effectively improved.
[0057] In some embodiments, ZrO 2 The sum of the mass percentages of BaO and ZnO is 0.2% to 3.2%, and ZrO 2 When the sum of the mass percentages of BaO and ZnO is within the above range, the glossiness, chemical stability and thermal stability of the base glass can be further increased.
[0058] In some embodiments, the raw material is composed of the following components, by weight percentage: 55% to 65% SiO 2 , 16.8%~21% Al 2 O 3 , 12% ~ 14.8% Na 2 O, 2.9% to 5% MgO, 0% to 3% K 2 O, 0-3% Li 2 O, 0~2.3% ZrO 2 , 0-3% B 2 O 3 , 0-1.5% BaO, 0-2% ZnO, and K 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages of ZrO is 3.2% to 5%. 2The sum of the mass percentages of BaO and ZnO is 0.2% to 3.2%.
[0059] In some embodiments, the raw material is composed of the following components, by weight percentage: 55% to 62.8% SiO 2 , 13% to 21% Al 2 O 3 , 12% ~ 15% Na 2 O, 2% to 5% MgO, 0 to 3% K 2 O, 0-1.6% Li 2 O, 0~2.3% ZrO 2 , 0.5% to 0.8% B 2 O 3 , 0-0.3% BaO, 0-2% ZnO, and K 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages of ZrO is 1.1% to 5%. 2 The sum of the mass percentages of BaO and ZnO is 0.2% to 4%.
[0060] In some embodiments, the raw material is composed of the following components, by weight percentage: 55% to 61.4% SiO 2 , 13% to 21% Al 2 O 3 , 14% ~ 15% Na 2 O, 2.1% to 4.5% MgO, 2.4% to 3% K 2 O, 0.2~2.3% ZrO 2 , 0.5% to 0.8% B 2 O 3 , 0~2% ZnO, and K 2 O. Li 2 O and B 2 O 3 The sum of the mass percentages of ZrO is 3.2% to 3.8%. 2 The sum of the mass percentages of BaO and ZnO is 0.2% to 4%.
[0061] The prepared raw materials are melted to convert the solid raw materials into a molten state to obtain a glass liquid with a certain viscosity. In some embodiments, the melting temperature is 1500°C to 1600°C and the time is 4h to 8h. Alternatively, the melting temperature is 1550°C to 1650°C and the time is 6h.
[0062] In some embodiments, after melting, the temperature is lowered to 1450° C. to 1550° C., and allowed to stand for 1 h to 5 h to homogenize the glass liquid.
[0063] In some embodiments, the molding method is selected from one of casting molding, float molding, calendaring molding, overflow molding and down-draw molding.
[0064] In some embodiments, the preparation method further comprises annealing the formed glass to obtain a base glass.
[0065] Step S200: performing a roughening treatment on a surface of the base glass to prepare a roughened glass.
[0066] During the roughening treatment, raised particles are formed on the surface of the base glass, and depressions are formed between adjacent particles, thereby forming an uneven texture on the base glass to achieve an anti-glare effect.
[0067] In some embodiments, the roughening treatment includes chemical etching treatment, frosting treatment and chemical polishing treatment in sequence. Through the above-mentioned roughening treatment, the surface of the base glass is roughened to form a dense, roughened surface with an anti-glare effect. Specifically, chemical etching treatment can cause the surface of the base glass to undergo an erosion reaction to form an uneven surface; frosting treatment is to crystallize the frosting powder on the eroded glass surface by immersion, forming a crystal nucleus and continuously growing, further improving the surface roughness of the base glass; chemical polishing treatment makes the uneven surface of the glass smoother, obtaining a uniform and delicate roughened surface.
[0068] In some embodiments, the etching solution used in the chemical etching process is a mixed solution of hydrofluoric acid and sulfuric acid, and the chemical etching process lasts for 10s to 60s. Optionally, the etching solution is a mixture of 6 vol% HF and 3 vol% H 2 SO 4 The mixed solution of 200 μg / ml and the chemical etching treatment time is 30 seconds. By adjusting the conditions of the chemical etching treatment, granular crystals are precipitated on the surface of the base glass, increasing the roughness and achieving an anti-glare effect.
[0069] In some embodiments, the frosting treatment uses a frosting liquid to immerse the base glass, and the frosting treatment time is 30s to 20s. Optionally, the frosting liquid is an aqueous solution containing frosting powder, the mass concentration of the frosting powder is 40% to 60%, and the frosting treatment time is 45s. By adjusting the conditions of the frosting treatment, granular crystals are further precipitated on the surface of the base glass to improve the roughness.
[0070] In some embodiments, the polishing liquid used in the chemical polishing process is a mixed solution of hydrofluoric acid and sulfuric acid, and the chemical polishing process lasts for 120s to 240s. Optionally, the etching solution is a mixture of 3 vol% HF and 2 vol% H 2 SO 4 The mixed solution of 200 μm and 200 μm was used, and the chemical etching time was 180 seconds. By adjusting the conditions of chemical polishing, the surface of the particles was made smoother and the clarity of the base glass was improved.
[0071] Step S300: heat-treating the roughened glass to flatten the surface of the particles, thereby preparing an anti-glare glass.
[0072] When roughened glass is heat-treated, it softens and its surface tension increases. At this time, the particles are deformed under the action of surface tension, increasing the size of the particles and making the surface smoother and glossier. And because the depressions between adjacent particles still exist, the roughened surface still has concave and convex textures, so it can meet the anti-glare requirements.
[0073] In some embodiments, the heat treatment includes: while heating the roughened glass, performing a pressing treatment. It is understandable that when the roughened glass is softened by heat, applying a certain external force to the surface of the roughened glass can make the deformation of the particles larger and further increase the size of the particles. And because the external force mainly acts on the top of the particles, the top of the particles can be smoothed downward, improving the flatness of the surface of the particles, thereby improving the glossiness of the anti-glare glass. The external force of the pressing treatment can come from an external pressing device, which has a component for controlling pressure and applying pressure; the external force of the pressing treatment can also come from the gravity of a pressing member set on the surface of the roughened glass. The specific components for implementing the pressing treatment in this application are not limited, and the anti-glare glass prepared can improve the flatness of the roughened surface while meeting the anti-glare requirements. In addition, the surface of the base glass that has not been roughened is subjected to a heat treatment, which can remove impurities on the surface, make it more flat and smooth, and thereby improve the overall glossiness of the anti-glare glass. It should be noted that the surface that has not been roughened is the surface of the base glass that is opposite to the roughened surface.
[0074] In some embodiments, the pressing process includes the following steps: a pressing piece having a smooth surface is respectively arranged on two surfaces of the roughened glass, and the smooth surface is in contact with the roughened glass. It can be understood that the smooth surface of the pressing piece is in contact with the surface of the roughened glass, which can improve the flatness and smoothness of the surface of the roughened glass. And because the pressing piece has a certain weight, it can apply a suitable pressure to the roughened glass, promote the smoothing of the top of the particles downward, and make different particles have similar protrusion heights, further improving the flatness of the roughened surface.
[0075] In some embodiments, the temperature of the thermal processing is 580° C. to 680° C. Optionally, the temperature is 580° C., 600° C., 620° C., 640° C., 660° C. or 680° C. It is understandable that the temperature of the thermal processing can also be selected in the range of 580° C. to 680° C.
[0076] In some embodiments, the temperature of the thermal treatment is 590° C. to 660° C., and optionally, the temperature is 590° C., 610° C., 630° C., 650° C. or 660° C. It is understandable that the temperature of the thermal treatment can also be selected in the range of 590° C. to 660° C. When the temperature of the thermal treatment is within the above range, the flatness of the particle surface can be further improved, and the glossiness of the anti-glare glass can be enhanced.
[0077] In some embodiments, the holding time of the heat treatment is 20 min to 50 min. Optionally, the holding time is 20 min, 25 min, 30 min, 35 min, 40 min, 45 min or 50 min. It is understandable that the holding time of the heat treatment can also be other suitable selections within the range of 20 min to 50 min.
[0078] In some embodiments, the preparation method further includes: obtaining the glossiness of the base glass after the roughening treatment, and determining the preset temperature according to the glossiness. Specifically, if the obtained glossiness is high, a lower temperature and a longer heat preservation time are selected for the heat treatment; if the obtained glossiness is low, a higher temperature and a shorter heat preservation time are selected for the heat treatment. According to the glossiness of the base glass after the roughening treatment, the temperature and heat preservation time of the heat treatment can be determined more accurately, the effect of the heat treatment can be improved, and the glossiness of the anti-glare glass can be further improved.
[0079] In some embodiments, the heating rate of the thermal treatment is 8°C / min to 15°C / min. Optionally, the heating rate is 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min or 15°C / min. It is understandable that the heating rate of the thermal treatment can also be selected in the range of 8°C / min to 15°C / min. By adopting a faster heating rate, the effect of the thermal treatment can be guaranteed.
[0080] In some embodiments, the preparation method further includes: before the roughening treatment, a protective film is provided on one surface of the base glass, and then the surface of the base glass facing away from the protective film is roughened. After the roughening treatment and before the heat treatment, the protective film is removed, and then the roughened glass is heat treated. It is understandable that during the roughening treatment, the side of the base glass provided with the protective film will not be roughened, while the surface of the side facing away from the protective film will be roughened, and a single-sided anti-glare roughened glass is formed after the heat treatment. The protective film needs to be removed before the heat treatment, that is, the heat treatment is performed on both surfaces of the roughened glass.
[0081] The method for preparing the anti-glare glass firstly prepares a base glass with high gloss, chemical temperature and thermal stability by adjusting the ratio of raw materials; then, the surface of the base glass is roughened to precipitate particles, forming a roughened surface with anti-glare effect, which effectively reduces the mirror reflection; and then, the roughened glass is softened by heat treatment to increase the surface tension of the roughened surface, thereby increasing the size of the particles and making the roughened surface smoother, so that the diffuse reflected light generated by the surface of the anti-glare glass is more orderly and the glossiness is increased. Thus, the anti-glare glass obtained has a high glossiness and a smoother surface while achieving the anti-glare effect. When used to prepare a display device, it can improve the visual effect and touch experience of the display device.
[0082] One embodiment of the present application provides an anti-glare glass, which is prepared according to the above-mentioned method for preparing the anti-glare glass.
[0083] In some embodiments, the anti-glare glass has a 60° gloss greater than or equal to 114%.
[0084] Finally, an embodiment of the present application further provides a display device, comprising the above-mentioned anti-glare glass. The above-mentioned display device includes but is not limited to a vehicle display screen, a mobile phone display screen or a computer display screen.
[0085] In order to make the purpose and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. The following are specific embodiments.
[0086] Examples 1 to 13 and Comparative Examples 1 to 3 are prepared according to the components in Tables 1 to 2, mixed evenly, placed in a platinum crucible, and melted at 1550°C to 1650°C for 6 hours, while stirring with a platinum stirring paddle. After the melting is completed, the platinum stirring paddle is pulled out, the temperature is lowered to 1450°C to 1550°C, kept warm for 2 hours, and homogenized to obtain glass liquid. It should be noted that the specific temperature of the above melting and the specific temperature of the cooling can be selected by those skilled in the art according to parameters such as the type and content of the raw materials. The glass liquid is then cast into an iron mold preheated to 500°C. After the glass liquid is hardened and formed, the obtained glass block is transferred to an annealing furnace for annealing for 6 hours, and the block-shaped basic glass is obtained after cooling. The above-mentioned block-shaped basic glass was cut into 70*140*1.1mm basic glass sheets using Shenyang Kejing's STX-1203 wire cutting machine, and then the basic glass sheets were thinned and polished using Shenzhen Hyde's HD-640-5L double-sided grinding and polishing machine, and then edge-grinded using CNC.
[0087] The processed base glass sheet is coated with an acid-resistant film (specifically, Nanning acid-resistant film) on one side, and the coated glass substrate is placed in a 6 vol% HF and 3 vol% H 2 SO 4 The glass substrate was then frosted with a frosting powder solution of 55% by mass for 45 seconds. After the treatment, it was washed with deionized water for 60 seconds, and then dried for use. The frosting powder was Jingermei high aluminum glass frosting powder. Then, 3 vol% HF and 2 vol% H were mixed in a volume ratio of 1:1. 2 SO 4 The glass substrate was chemically polished with a mixture of , the treatment time was 180s, and after the treatment was completed, it was washed with deionized water for 120s, and then dried for use. The 60° glossiness of the roughened surface of the base glass sheet after the roughening treatment was tested using an IQ 20 / 60 / 85 haze meter, and the test results are shown in Tables 1 and 2.
[0088] The temperature and holding time of the heat treatment are determined according to the test results of the above 60° glossiness. The specific temperature and holding time are shown in Tables 1-2. Tear off the acid-resistant film on the base glass sheet, and place two quartz polishing sheets on the two opposite surfaces of the above base glass sheet, so that the base glass sheet is clamped between the two quartz polishing sheets, and then the three are placed together in a Sigma box-type resistance furnace (model SGM.M12 / 12A). Then heat up to the preset temperature at a rate of 10°C / min, and then keep warm. After the heat treatment, cool naturally to obtain anti-glare glass. Test the 60° glossiness of the roughened surface of the above anti-glare glass, and the test results are shown in Tables 1-2.
[0089] The surface particles of Example 1 after roughening treatment and heat treatment were observed using a Leica polarizing microscope DM2700P. Figure 1 This is a polarizing microscope image of the roughened surface of the product after roughening treatment. Figure 2 for Figure 1 A partial enlarged view of Figure 3 This is a polarizing microscope image of the roughened surface of the product after roughening and heat treatment. Figure 4 for Figure 3 A partial enlarged view of the Figure 2 The sizes are: 1.L: 4.351μm, 2.L: 4.485μm, 3.L: 4.343μm; Figure 4 The dimensions are: 1.L: 5.087μm, 2.L: 4.954μm, 3.L: 5.259μm. Figure 1 and Figure 3 It can be seen from the comparison that after heat treatment, the surface of the particles is smoother and the transition between particles is smoother. Figure 2 and Figure 4 It can be seen from the comparison that heat treatment increases the average particle size of the roughened surface particles.
[0090] Table 1
[0091]
[0092] Table 2
[0093]
[0094]
[0095] Please refer to Tables 1-2. The anti-glare glass of Examples 1-13 comprises, by mass percentage, 55% to 65% SiO 2 , 12%~21% Al 2 O 3 , 12% ~ 16% Na 2 O, 2% to 5% MgO, 0 to 3% K 2 O, 0-3% Li 2 O, 0-1.5% ZrO, 0-3% B 2 O 3 , 0~1.5% BaO, 0~2% ZnO. And BaO, ZrO 2 The sum of the mass percentages of K and ZnO does not exceed 5%; 2 O. Li 2 O and B 2 O 3The sum of the mass percentages of BaO and ZrO does not exceed 5%. 2 , ZnO, K 2 O. Li 2 O and B 2 O 3 At least one of the above improves the optical properties of the base glass and enhances the glossiness of the base glass itself. After roughening, the base glass achieves an anti-glare function. After chemical polishing, the 60° glossiness can reach 103%. After thermal processing, the 60° glossiness is further improved. The display device prepared by the above anti-glare glass has a good visual effect.
[0096] Compared with Example 5, the temperature of the heat treatment of Example 11 is lower. Although the heat preservation time is extended, the 60° gloss of Example 11 is still lower than that of Example 5. Compared with Example 2, the temperature of the heat treatment of Example 12 is higher. Although its 60° gloss is also slightly higher than that of Example 2, there are fine stripes on its surface. When used to prepare a display device, it will cause image distortion and affect the visual effect. The above results show that when the preset temperature of the heat treatment is 580℃~680℃, the gloss of the product can be further improved.
[0097] Compared with Example 8, the holding time of Example 13 is shorter, and its 60° gloss is also lower than that of Example 8, indicating that when the holding time of the heat treatment is too short, the flatness of the particle surface cannot be effectively improved, and the surface of the anti-glare glass is still relatively rough. The improvement of the gloss by the heat treatment is small, that is, when the holding time of the heat treatment meets the requirements of 20min to 50min, the gloss of the product can be further improved.
[0098] In Comparative Example 1, Na 2 O exceeds 16.0%, resulting in poor thermal and chemical stability of the base glass; and without adding the above-mentioned BaO, ZrO 2 , ZnO, K 2 O. Li 2 O and B 2 O 3 In any of the above examples, the base glass sheet itself has a poor glossiness. After roughening and heat treatment, the 60° glossiness is only 94%. 2 O 3 The content of BaO and ZrO is not within the scope of this application, the melting temperature of the glass raw materials is high, which makes the performance of the obtained basic glass worse; and the above-mentioned BaO, ZrO 2 , ZnO, K 2 O. Li 2 O and B 2 O 3In any of the above, the base glass sheet itself has poor glossiness. After subsequent treatment, the 60° glossiness is only 88%. 2 When the sum of the mass percentages of ZnO and ZnO is greater than 5%, crystallization is likely to occur during the preparation of the base glass, and the surface properties of the base glass are changed. As a result, it is not easy to adsorb frosting powder during frosting treatment, and fewer crystals are formed. Therefore, the glossiness of the comparative example is reduced and the anti-glare effect is poor.
[0099] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0100] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.
Claims
1. A method for preparing anti-glare glass, characterized in that: The steps include: Melt and shape the raw materials to prepare basic glass; Roughening a surface of the base glass to prepare a roughened glass; The roughened glass is subjected to heat treatment to make the roughened surface of the roughening treatment flat, so as to prepare anti-glare glass; the temperature of the heat treatment is 610° C. to 640° C.; the heat preservation time of the heat treatment is 20 min to 45 min; Wherein, the raw materials include the following components in terms of mass percentage: The sum of the mass percentages of K2O, Li2O and B2O3 is 3.2% to 5%, and the sum of the mass percentages of ZrO2, BaO and ZnO is 2.5% to 3.2%.
2. The method for preparing anti-glare glass according to claim 1, characterized in that: The mass percentage of the Na2O is 12% to 14.8%.
3. The method for preparing anti-glare glass according to claim 1, characterized in that: The mass percentage of the MgO is 2.9% to 5%.
4. The method for preparing anti-glare glass according to claim 1, characterized in that: The roughening treatment includes chemical etching treatment, frosting treatment and chemical polishing treatment performed in sequence.
5. The method for preparing anti-glare glass according to any one of claims 1 to 4, characterized in that: The thermal processing includes: performing a pressing process while heating the roughened glass.
6. The method for preparing anti-glare glass according to claim 5, characterized in that: The pressing process comprises the following steps: Pressed parts with smooth surfaces are respectively arranged on two surfaces of the roughened glass, and the smooth surfaces are in contact with the roughened glass.
7. The method for preparing anti-glare glass according to any one of claims 1 to 4, characterized in that: The heating rate of the thermal treatment is 8°C / min to 15°C / min.
8. The method for preparing anti-glare glass according to any one of claims 1 to 4, characterized in that: The preparation method also includes: before the roughening treatment, providing a protective film on one surface of the base glass, and then performing the roughening treatment on the surface of the base glass facing away from the protective film; and after the roughening treatment and before the heat treatment, removing the protective film, and then performing the heat treatment on the roughened glass. 9.An anti-glare glass, characterized in that: The anti-glare glass is prepared according to the method for preparing the anti-glare glass according to any one of claims 1 to 8, wherein the 60° glossiness of the anti-glare glass is greater than or equal to 142%.
10. A display device, characterized in that: Including the anti-glare glass as described in claim 9.
Citation Information
Patent Citations
Low sparkle glass sheet
CN106470954A
Polishing solution and production process for AG (Anti-glare) glass
CN106892572A
Manufacturing method of anti-glare cover plate
CN112661410A
Anti-blue-light high-strength lithium-aluminum-silicon cover plate glass and preparation method and application thereof
CN113121109A
Polishing solution for display frosted glass and application thereof
CN114772941A