A modified rice husk fiber toughening grouting material and preparation method thereof
The combination of rice husk fiber modified by acid-base purification, silane coupling agent and fly ash solves the brittleness and dry shrinkage of traditional grouting materials in high stress environments, and improves the toughness and resistance of grouting materials. The disturbance capability achieves a low-carbon and environmentally friendly grouting effect.
Patent Information
- Application Number
- CN202310393131.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-13
AI Technical Summary
Traditional grouting materials are prone to dry shrinkage, brittleness and poor toughness in high ground stress, high ground temperature, high osmosis pressure and strong mining disturbance environments. The direct use of rice husk fiber in cement grouting materials will affect the strength of the specimen. and stability.
The modified rice husk fibers were extracted and surface modified by acid-base purification, combined with silane coupling agent and fly ash to form a modified rice husk fiber toughening grouting material. The gelling time and toughness were controlled through a double-liquid grouting pump. .
Improve the toughness, crack resistance, disturbance resistance and durability of grouting materials, reduce material density, enhance the integrity and compressive strength of surrounding rocks, reduce carbon emissions, and achieve low-cost and environmentally friendly grouting effect. .
Smart Images

Figure CN116283201B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical fields of agricultural product waste treatment and secondary utilization, solid waste treatment, and new grouting material research and development, in particular to a modified rice husk fiber toughening grouting material and a preparation method thereof. Background Art
[0002] Most traditional grouting materials are brittle, prone to shrinkage after solidification, and have poor toughness. With the advancement of mineral resource development in my country, the development of deep stratum resources has become increasingly important. However, with the continuous increase in mining depth, the surrounding rock of deep tunnels has shown soft rock characteristics, and often has environmental problems such as high ground stress, high ground temperature, high osmotic pressure and strong mining disturbance, making mining difficult. In order to eliminate the safety problems caused by surrounding rock damage, surrounding rock grouting reinforcement is one of the effective methods of tunnel support, especially soft rock tunnel support. Through grouting construction, the originally loose surrounding rock can be consolidated into a whole to enhance its stability. During the entire construction process, the characteristics of the grouting material greatly affect the grouting effect. In actual projects, the most commonly used inorganic materials are cement, cement-water glass, etc. However, due to their low bonding strength, small diffusion radius and poor toughness, they are used in some loose and broken soft rock geology. Although they have a certain reinforcement effect in the early stage, the stone body is prone to shrinkage in the later stage, and then tiny cracks will appear, which will destroy the integrity of the stone body and the surrounding rock, and the reinforcement effect will be significantly weakened, and the anti-interference ability is poor.
[0003] Similarly, rice husk, a byproduct of rice processing in my country, has an annual output of tens of millions of tons, which is a huge renewable resource. However, the current means of processing and utilizing rice husk are relatively simple, mostly landfilling as waste, incinerating as fuel, and using as feed raw materials. There are few cases of using rice husk in cement materials. The reason is that rice husk is very hydrophilic. If rice husk is directly added to cement grouting materials, the rice husk inside the slurry will absorb the surrounding free water and expand, causing the incomplete bond between the rice husk and the matrix interface to be destroyed, thereby affecting the overall strength of the specimen. Moreover, after the rice husk meets water, the lignin, pentosan, etc. in the leachate are adsorbed together with the cement hydration products, changing the properties of the surface of the gel particles. The ion exchange increases the double-layer potential of the contact surface, and the surface tension of the particles is enhanced, which enhances the stability of the gel system and leads to a slow setting effect. In addition, the rice husk leachate will also have an anti-coagulation effect on the hydration reaction, which in turn affects the strength of the specimen. Therefore, if untreated rice husks are directly used in grouting materials, it will affect the strength and other properties of the material. However, if the rice husk fibers in the rice husks are extracted and modified by acid-base purification methods and then added to cement grouting materials, the toughness and anti-disturbance ability of the grouting materials can be further enhanced.
[0004] Therefore, under the background of the current "double carbon" plan, the acid-base purification method is used to extract and modify rice husk fiber, giving full play to the advantages of rice husk fiber such as good toughness, and applying it to grouting materials. On the one hand, it can reduce the pollution caused by rice husk burning, effectively improve its utilization rate, and achieve the purpose of carbon reduction; on the other hand, it can further improve the toughness of grouting materials, make up for the shortcomings of traditional grouting materials, and provide new ideas for the research and development of grouting materials. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a modified rice husk fiber toughened grouting material and a preparation method thereof. The prepared modified rice husk fiber toughened grouting material has high injectability, strong diffusion ability, good pumping stability, controllable gelation time, good stone body toughness, good crack resistance, good anti-disturbance ability, good tensile performance, high durability, environmental friendliness, low carbon and environmental protection, and low cost.
[0006] To achieve the above object, the present invention is implemented according to the following technical solutions:
[0007] The first object of the present invention is to provide a modified rice husk fiber toughening grouting material, which is mixed with liquid A and liquid B in a volume ratio of 1:0.53 to 1:0.76, wherein the liquid A is composed of the following components in parts by weight: 400 parts of cement, 5 to 20 parts of modified rice husk fiber, 5 to 10 parts of silane coupling agent, 10 to 20 parts of early strength agent, and 300 parts of water; the liquid B is composed of the following components in parts by weight: 150 parts of sodium silicate, 320 parts of fly ash, and 300 parts of water.
[0008] Furthermore, the modified rice husk fiber is a rice husk fiber extracted and surface-modified by an acid-base purification method, and the specific steps for preparing the modified rice husk fiber are:
[0009] 1) Take 40 parts of rice husks by weight and place them in a JC-FW-400A grinding mill with a grinding fineness of 40-200 meshes. Set the working time to 3 minutes. During the grinding process, tilt the grinder 45 degrees back and forth every 2-5 seconds to fully grind the rice husks to obtain rice husk powder within the required particle size range;
[0010] 2) passing the rice husk powder obtained in step 1) through a 0.5 mm sieve to obtain rice husk powder with a particle size of ≤0.5 mm;
[0011] 3) The rice husk powder with a particle size of ≤0.5 mm obtained in step 2) is completely immersed in a H2SO4 solution with a concentration of 8% to 10%, and the temperature is controlled at 45 to 55° C. in a constant temperature water bath for acid leaching for 40 to 50 minutes, and then the acid-leached rice husk powder is filtered out, and rinsed with water until the pH value is neutral; then the acid-leached rice husk powder is completely immersed in a NaOH solution with a concentration of 8% to 10%, and the temperature is controlled at 80 to 90° C. in a constant temperature water bath for alkali leaching for 80 to 90 minutes, and then the alkali-leached rice husk powder is filtered out, and rinsed with water until the pH value is neutral to obtain rice husk fiber powder;
[0012] 4) The rice husk fiber powder obtained in step 3) is dried in a drying oven for 8 hours at a temperature set at 80° C. to 105° C., and then sieved through a 250 μm sieve and a 150 μm sieve in sequence. The rice husk fiber remaining on the 150 μm sieve is the modified rice husk fiber.
[0013] Preferably, the particle size of the modified rice husk fiber is 150-250 μm.
[0014] Preferably, the silane coupling agent includes but is not limited to KH550 silane coupling agent, KH602 silane coupling agent, and KH-792 silane coupling agent.
[0015] Preferably, the early strength agent includes but is not limited to calcium chloride, triethanolamine, calcium nitrite-calcium nitrate.
[0016] Preferably, the fly ash includes but is not limited to Class C fly ash from burning lignite or sub-bituminous coal, and high-calcium fly ash.
[0017] Preferably, the cement is ordinary Portland cement with a strength of not less than 42.5.
[0018] Preferably, the concentration of the sodium silicate is 40°Bé.
[0019] The second object of the present invention is to provide a method for preparing a modified rice husk fiber toughened grouting material, comprising the following steps:
[0020] Step 1: fully mix the cement, modified rice husk fiber, silane coupling agent and early strength agent in liquid A in a mixer according to weight proportions, stir evenly, control the temperature to be 23°C to 40°C, the humidity to be 35% to 55%, the stirring speed to be 100 to 120 r / min, and the stirring time to be 5 to 10 min during stirring;
[0021] Step 2: fully mix the sodium silicate and fly ash and other raw materials in liquid B in a mixer according to their weight proportions, stir evenly, control the temperature to be 23°C to 40°C, the humidity to be 35% to 55%, the stirring speed to be 120 to 150 r / min, and the stirring time to be 3 to 8 min during stirring;
[0022] Step 3, adding water by weight to the raw material mixtures A and B obtained in steps 1 and 2, respectively, and placing them in a blender and stirring them evenly to obtain liquid A and liquid B; during stirring, the temperature is controlled to be 23°C to 40°C, the humidity is 35% to 55%, the stirring rate is 120 to 150 r / min, and the stirring time is 5 to 10 min;
[0023] Step 4: Use a double-liquid grouting pump to mix the liquid A and liquid B obtained in step 3 at a volume ratio of 1:0.53 to 1:0.76, and stir evenly to obtain the modified rice husk fiber toughening grouting material.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] First, rice husk fiber has excellent crack resistance and strengthening effects. It can not only greatly reduce the original cracks inside the grouting material body, but also effectively prevent the initiation and expansion of cracks, transform brittle failure into ductile fracture, and improve the tensile performance and toughness of the grouting material body. In the early stage of loading (tension and bending), the cement and fiber in the grouting material body bear the external force together, and the former is the main force bearer; when cracking occurs, the fiber across the crack becomes the main bearer of external force, that is, the bridging force of the fiber is mainly used to resist the external force. If the volume content of the fiber is greater than a certain critical value, the entire composite material can continue to bear a higher load and produce a larger deformation until the fiber is broken or pulled out of the matrix. Rice husk fiber has good tensile properties. After being added to the grouting material, it can significantly improve its tensile, bending, shear and other mechanical properties, as well as long-term mechanical properties such as crack resistance. In particular, rice husk fiber with high elastic modulus can also greatly enhance the fracture toughness and impact resistance of the grouting material and improve the toughness of the material.
[0026] Second, after the rice husk fiber toughened grouting material is pressed into the soft and broken surrounding rock, it will continue to penetrate into the rock layer along the cracks, forming a vein structure similar to the plant root system, enveloping the soft and broken rocks around it, enhancing the integrity of the surrounding rock to strengthen the surrounding rock. At the same time, although the addition of rice husk fiber reduces the density of the grouting material stone body, it further improves its toughness and anti-disturbance ability, thereby improving the toughness and anti-disturbance ability of the surrounding rock. Under the action of external loads, the soft and broken surrounding rock is able to undergo a certain elastic deformation, especially under compression. The internal structure of the grouting material stone body is further compacted, the density is increased, and the compressive resistance is improved, thereby ensuring the compressive strength of the surrounding rock; and in the face of some concentrated stress damage, the toughness and integrity of the surrounding rock after grouting can be fully utilized to disperse the concentrated stress and bear the force as a whole. As a result, the tensile strength, toughness and integrity of the soft and broken surrounding rock are greatly improved.
[0027] Third, the general formula of the added silane coupling agent is RSiX3. According to the characteristics of the molecular structure, R is an organic-philic group that can react with rice husk fibers on the surface; X is a hydrolyzable group that can react chemically with the surface of cement particles. The coupling agent is dissolved in water and undergoes hydrolysis to generate monomers and oligomers. The oligomers form hydrogen bonds with the -OH on the surface of cement particles, and after drying and condensation, they form M-O-Si covalent bonds with the cement surface. The organic group R in the silane coupling layer covering the cement surface finally expands into the polymer and undergoes a cross-linking reaction with the rice husk fibers at the interface to form silicon-oxygen bonds, so that the rice husk fibers and cement particles are fully bonded.
[0028] Fourth, in the preparation process of rice husk fiber toughened grouting material, a scientific and reasonable method is adopted to extract rice husk fiber from rice husk and modify its surface, and then add it into the grouting material for toughening, thereby reducing the CO2 generated by burning rice husk, which is in line with the concept of low carbon and environmental protection; and it turns waste into treasure, solving the problems of the anti-coagulation effect of directly adding original rice husk on cement grouting material and the adverse effect on the strength of the stone body.
[0029] Fifth, by utilizing the particle morphology effect and micro-aggregate effect of high calcium fly ash, when liquid A and liquid B are mixed, the fly ash is evenly distributed in the system, filling the gaps and pores, improving the pore structure of the system, increasing the density of the slurry, and improving the impermeability of the material. At the same time, in liquid B, the activation effect of sodium silicate on fly ash is utilized to increase the amount of gel material and improve the quality of gel material, thus solving the problem of excessive sodium silicate relative to cement in cement-water glass slurry. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention is a flow chart of the preparation method of the modified rice husk fiber toughening grouting material. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the invention.
[0032] Example 1
[0033] The modified rice husk fiber toughening grouting material of this embodiment is mixed with liquid A and liquid B in a volume ratio of 1:0.75, wherein liquid A is composed of the following components: 400 g of ordinary Portland cement, 8 g of modified rice husk fiber, 10 g of silane coupling agent, 16 g of calcium chloride, and 300 g of water; liquid B is composed of the following components: 150 g of sodium silicate (concentration of 40°Bé), 320 g of fly ash, and 300 g of water.
[0034] Example 2
[0035] The modified rice husk fiber toughening grouting material of this embodiment is mixed with liquid A and liquid B in a volume ratio of 1:0.75, wherein liquid A consists of the following components: 400 g of ordinary Portland cement, 17 g of modified rice husk fiber, 10 g of silane coupling agent, 16 g of calcium chloride, and 300 g of water; liquid B consists of the following components: 150 g of sodium silicate, 320 g of fly ash, and 300 g of water.
[0036] like Figure 1 As shown, the method for preparing the modified rice husk fiber grouting material described in Example 1 and Example 2 comprises the following specific steps:
[0037] Step 1: Mix the required ordinary Portland cement, rice husk fiber, silane coupling agent, calcium chloride and other raw materials in liquid A in a mixer according to their weight parts, stir evenly, control the temperature at 23°C to 40°C, the humidity at 35% to 55%, the stirring speed at 120r / min, and the stirring time at 8min.
[0038] Step 2: Mix the sodium silicate required in liquid B with high-calcium fly ash and other raw materials in a mixer according to their weight proportions and stir evenly. During stirring, control the temperature to 23°C to 40°C, the humidity to 35% to 55%, the stirring speed to 130r / min, and the stirring time to 5min.
[0039] Step 3: Add water by weight to the raw material mixtures A and B obtained in steps 1 and 2 respectively, mix them thoroughly in a blender, stir them evenly, control the temperature to 23°C to 40°C, the humidity to 35% to 55%, the stirring rate to 130r / min, and the stirring time to 10min during stirring to obtain liquid A and liquid B.
[0040] Step 4: Use a double-liquid grouting pump to mix the liquid A and liquid B obtained in step 3 at a volume ratio of 1:0.75, and stir evenly to obtain the rice husk fiber toughening grouting material.
[0041] Among them, the modified rice husk fiber is extracted by acid-base purification method and surface modified, and the specific steps are:
[0042] Step 1: Take 40 parts of rice husks by weight and put them into a JC-FW-400A grinding mill with a grinding fineness of 40-200 meshes. Set the working time to 3 minutes. During the grinding process, tilt the grinder 45 degrees back and forth every 2-5 seconds to fully grind the rice husks to obtain rice husk powder within the required particle size range;
[0043] Step 2: Pass the rice husk powder obtained in step 1 through a 0.5 mm sieve to obtain rice husk powder with a particle size of ≤0.5 mm.
[0044] Step 3: Extract and surface modify rice husk fiber. Add 8% H2SO4 solution to the rice husk powder with a particle size of ≤0.5mm obtained in step 2 to immerse the rice husk powder, control the temperature at 45°C in a constant temperature water bath for 40 minutes, stir every 10 to 15 minutes during the immersion process, the stirring rate is 50r / min, and the stirring time is 3 to 5 minutes to dissolve the lignin and pectin in the rice husk and retain the rice husk fiber; then filter out the soaked rice husk powder, rinse with water until the pH value is close to 7, and obtain rice husk fiber powder; then add 8% NaOH solution to the rice husk fiber powder to immerse the rice husk fiber powder, control the temperature at 80°C in a constant temperature water bath for 90 minutes to modify the surface of the rice husk fiber; finally, rinse the modified rice husk fiber powder with water until the pH value is close to 7.
[0045] Step 4: Dry the rice husk fiber powder obtained in step 3 in a drying oven for 8 hours at a temperature set at 105°C, then pass it through a 250 μm sieve and a 150 μm sieve in turn, and take the rice husk fiber remaining on the 150 μm sieve as the modified rice husk fiber.
[0046] Example 3
[0047] The difference from Example 1 is that, the modified rice husk fiber is extracted by acid-base purification method and surface modified, and the specific steps are as follows:
[0048] Step 1: Take 40 parts of rice husks by weight and put them into a JC-FW-400A grinding mill with a grinding fineness of 40-200 meshes. Set the working time to 3 minutes. During the grinding process, tilt the grinder 45 degrees back and forth every 2-5 seconds to fully grind the rice husks to obtain rice husk powder within the required particle size range;
[0049] Step 2: Pass the rice husk powder obtained in step 1 through a 0.5 mm sieve to obtain rice husk powder with a particle size of ≤0.5 mm.
[0050] Step 3: Extract and surface modify rice husk fiber. Add 10% H2SO4 solution to the rice husk powder with a particle size of ≤0.5mm obtained in step 2 to immerse the rice husk powder, control the temperature at 55°C in a constant temperature water bath for 50 minutes, stir every 10 to 15 minutes during the immersion process, the stirring rate is 40 to 60r / min, and the stirring time is 3 to 5 minutes to dissolve the lignin and pectin in the rice husk and retain the rice husk fiber; then filter out the soaked rice husk powder, rinse with water until the pH value is close to 7, and obtain rice husk fiber powder; then add 10% NaOH solution to the rice husk fiber powder to immerse the rice husk fiber powder, control the temperature at 90°C in a constant temperature water bath for 90 minutes to modify the surface of the rice husk fiber; finally, rinse the modified rice husk fiber powder with water until the pH value is close to 7.
[0051] Step 4: Dry the rice husk fiber powder obtained in step 3 in a drying oven for 8 hours at a temperature set at 105°C, then pass it through a 250 μm sieve and a 150 μm sieve in turn, and take the rice husk fiber remaining on the 150 μm sieve as the modified rice husk fiber.
[0052] Example 4
[0053] The difference from Example 2 is that: wherein the modified rice husk fiber is extracted by acid-base purification method and surface modified, and the specific steps are:
[0054] Step 1: Take 40 parts of rice husks by weight and put them into a JC-FW-400A grinding mill with a grinding fineness of 40-200 meshes. Set the working time to 3 minutes. During the grinding process, tilt the grinder 45 degrees back and forth every 2-5 seconds to fully grind the rice husks to obtain rice husk powder within the required particle size range;
[0055] Step 2: Pass the rice husk powder obtained in step 1 through a 0.5 mm sieve to obtain rice husk powder with a particle size of ≤0.5 mm.
[0056] Step 3: Extract and surface modify rice husk fiber. Add 10% H2SO4 solution to the rice husk powder with a particle size of ≤0.5mm obtained in step 2 to immerse the rice husk powder, control the temperature at 55°C in a constant temperature water bath for 50 minutes, stir every 10 to 15 minutes during the immersion process, the stirring rate is 40 to 60r / min, and the stirring time is 3 to 5 minutes to dissolve the lignin and pectin in the rice husk and retain the rice husk fiber; then filter out the soaked rice husk powder, rinse with water until the pH value is close to 7, and obtain rice husk fiber powder; then add 10% NaOH solution to the rice husk fiber powder to immerse the rice husk fiber powder, control the temperature at 90°C in a constant temperature water bath for 90 minutes to modify the surface of the rice husk fiber; finally, rinse the modified rice husk fiber powder with water until the pH value is close to 7.
[0057] Step 4: Dry the rice husk fiber powder obtained in step 3 in a drying oven for 8 hours at a temperature set at 105°C, then pass it through a 250 μm sieve and a 150 μm sieve in turn, and take the rice husk fiber remaining on the 150 μm sieve as the modified rice husk fiber.
[0058] Comparative Example 1
[0059] The components and weight proportions are: Liquid A: 400g of ordinary Portland cement, 16g of calcium chloride, 300g of water; Liquid B: 150g of sodium silicate, 320g of fly ash, 300g of water. Rice husk fiber extracted and surface-modified by acid-base purification method and the required silane coupling agent are not added.
[0060] The grouting material preparation method described in Comparative Example 1 comprises the following specific steps:
[0061] Step 1: Mix the required ordinary Portland cement, calcium chloride and other raw materials in liquid A in a mixer according to their weight proportions, stir evenly, control the temperature at 23°C to 40°C, the humidity at 35% to 55%, the stirring speed at 120r / min, and the stirring time at 8min.
[0062] Step 2: Mix the sodium silicate required in liquid B with high-calcium fly ash and other raw materials in a mixer according to their weight proportions and stir evenly. During stirring, control the temperature to 23°C to 40°C, the humidity to 35% to 55%, the stirring speed to 130r / min, and the stirring time to 5min.
[0063] Step 3: Add water by weight to the raw material mixtures A and B obtained in steps 1 and 2 respectively, mix them thoroughly in a blender, stir them evenly, control the temperature to 23°C to 40°C, the humidity to 35% to 55%, the stirring rate to 130r / min, and the stirring time to 10min during stirring to obtain liquid A and liquid B.
[0064] Step 4: Use a double-liquid grouting pump to mix the liquid A and liquid B obtained in step 3 at a volume ratio of 1:0.75, and stir evenly to obtain the grouting material.
[0065] The grouting materials prepared in the above-mentioned Examples 1, 2, 3, 4 and Comparative Example 1 were respectively tested for basic properties such as density, viscosity, gel time, stone rate, and permeability coefficient, as well as toughness properties such as flexural strength, maximum strain before peak, maximum strain after peak, elastic modulus, and compressive strength of the stone body after curing for 28 days. The determination methods are all conventional detection methods for the above-mentioned parameters of the grouting materials, and the determination results are shown in Tables 1 and 2.
[0066] Table 1
[0067]
[0068] Table 2
[0069]
[0070] It can be seen from the data in Table 1 that both the embodiments and the comparative examples meet the basic performance requirements of the grouting materials, and the addition of rice husk fibers does not affect the injectability of the grouting materials. By comparing Examples 1, 2, 3, and 4 with Comparative Example 1, it can be seen that after the addition of rice husk fibers, the stone rate of the grouting material is reduced, indicating that the amount of slurry water separation during the solidification process of the grouting material of the invention is reduced, and the addition of fibers improves the shrinkage of traditional cement grouting materials to a certain extent.
[0071] It can be seen from the data in Table 2 that, with the addition of rice husk fiber obtained by the same preparation method, as the amount of rice husk fiber increases, the compressive strength of the material is slightly weakened, and the toughness is improved; the data obtained from the comparative examples 1, 3, 2, and 4 show that the grouting material with the same amount of rice husk fiber, as the acid-base concentration, soaking temperature and time increase during the preparation of rice husk fiber, the compressive strength and toughness of the material are improved. It can be seen that the obtained rice husk fiber is purer and the surface modification is better. The data obtained from the comparative examples 1, 2, 3, and 4 show that the rice husk fiber toughened grouting material still has a high compressive strength, but the toughness has been greatly improved. The material has a controllable gelation time, good stone toughness, good crack resistance, good anti-disturbance ability, good tensile performance, high durability, environmental friendliness, low carbon and low cost.
[0072] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.
Claims
1. A modified rice husk fiber toughening grouting material, characterized in that: The mixture is prepared by mixing liquid A and liquid B in a volume ratio of 1:0.53 to 1:0.76, wherein the liquid A is composed of the following components in parts by weight: 400 parts of cement, 5 to 20 parts of modified rice husk fiber, 5 to 10 parts of silane coupling agent, 10 to 20 parts of early strength agent, and 300 parts of water; the liquid B is composed of the following components in parts by weight: 150 parts of sodium silicate, 320 parts of fly ash, and 300 parts of water; The modified rice husk fiber is obtained by extracting and surface-modifying the rice husk fiber using an acid-base purification method. The specific steps for preparing the modified rice husk fiber are as follows: 1) Take 40 parts of rice husk by weight and place them in a JC-FW-400A grinding mill with a grinding fineness of 40-200 mesh. Set the working time to 3 minutes. During the grinding process, tilt the grinder 45 degrees back and forth every 2-5 seconds to fully grind the rice husk to obtain rice husk powder within the required particle size range; 2) passing the rice husk powder obtained in step 1) through a 0.5 mm sieve to obtain rice husk powder with a particle size of ≤0.5 mm; 3) The rice husk powder with a particle size of ≤0.5 mm obtained in step 2) is completely immersed in a H2SO4 solution with a concentration of 8% to 10%, and the temperature is controlled at 45 to 55° C. in a constant temperature water bath for acid leaching for 40 to 50 minutes, and then the acid-leached rice husk powder is filtered out, and rinsed with water until the pH value is neutral; then the acid-leached rice husk powder is completely immersed in a NaOH solution with a concentration of 8% to 10%, and the temperature is controlled at 80 to 90° C. in a constant temperature water bath for alkali leaching for 80 to 90 minutes, and then the alkali-leached rice husk powder is filtered out, and rinsed with water until the pH value is neutral to obtain rice husk fiber powder; 4) The rice husk fiber powder obtained in step 3) is dried in a drying oven for 8 hours at a temperature set at 80°C to 105°C, and then passed through a 250 μm sieve and a 150 μm sieve in sequence. The rice husk fiber remaining on the 150 μm sieve is the modified rice husk fiber.
2. The modified rice husk fiber toughening grouting material according to claim 1, characterized in that: The silane coupling agent includes KH550 silane coupling agent, KH602 silane coupling agent and KH-792 silane coupling agent.
3. The modified rice husk fiber toughening grouting material according to claim 1, characterized in that: The early strength agent includes calcium chloride, triethanolamine, calcium nitrite-calcium nitrate.
4. The modified rice husk fiber toughening grouting material according to claim 1, characterized in that: The fly ash includes Class C fly ash and high-calcium fly ash obtained by burning lignite or sub-bituminous coal.
5. The modified rice husk fiber toughening grouting material according to claim 1, characterized in that: The cement is ordinary Portland cement with a strength of not less than 42.
5.
6. The modified rice husk fiber toughening grouting material according to claim 1, characterized in that: The concentration of the sodium silicate is 40° Bé.
7. A method for preparing the modified rice husk fiber toughened grouting material according to claim 1, characterized in that: The following steps are involved: Step 1: fully mix the cement, modified rice husk fiber, silane coupling agent and early strength agent required in liquid A in a mixer according to weight proportions, stir evenly, control the temperature to be 23°C to 40°C, the humidity to be 35% to 55%, the stirring speed to be 100 to 120 r / min, and the stirring time to be 5 to 10 min during stirring; Step 2: fully mix the sodium silicate required in liquid B and the fly ash raw material in a mixer according to the weight ratio, stir evenly, control the temperature to be 23°C to 40°C, the humidity to be 35% to 55%, the stirring speed to be 120 to 150 r / min, and the stirring time to be 3 to 8 min during stirring; Step 3, adding water by weight to the raw material mixtures A and B obtained in steps 1 and 2, respectively, and placing them in a blender and stirring them evenly to obtain liquid A and liquid B; during stirring, the temperature is controlled to be 23°C to 40°C, the humidity is 35% to 55%, the stirring rate is 120 to 150 r / min, and the stirring time is 5 to 10 min; Step 4: Mix the liquid A and liquid B obtained in step 3 in a volume ratio of 1:0.53-1:0.76, and stir evenly to obtain the modified rice husk fiber toughening grouting material.