Preparation method and application of nano-transition metal oxide modified flat ceramic membrane
By uniformly growing nano-scale transition metal oxides on the surface of ceramic particles inside the ceramic membrane, the problems of surface pore blockage and catalytic reaction limitations during the catalytic degradation of ceramic membranes are solved, and efficient degradation of macromolecular pollutants and water flux are achieved. Maintaining, significantly improving catalytic performance and stability.
Patent Information
- Application Number
- CN202310292168.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-23
AI Technical Summary
During the catalytic degradation process, existing ceramic membranes are prone to surface hole blockage, water flux decreases, and catalytic reactions are limited to the membrane surface, which has poor degradation effect on small-molecular pollutants and is difficult to effectively treat concentrated liquids with high concentrations of pollutants.
Complexing agent-assisted impregnation-calcination method is used to uniformly grow nano-scale transition metal oxides on the surface of ceramic particles inside the flat-panel ceramic membrane to form a catalytic film. The nano-transition metal oxides are fixed by low-temperature calcination, maintain the water flux of the ceramic membrane and achieve large amounts. Effective degradation of molecular pollutants.
It realizes efficient catalytic degradation of carbamazepine antibiotics in water bodies, maintains high water flux, stable and long-term effective catalytic performance, can treat macromolecular pollutants in the presence of persulfate, and is not easy to cause membrane pore blockage. .
Smart Images

Figure CN116283359B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation and application of water treatment catalytic ceramic membranes, and in particular to a preparation method and application of a nano transition metal oxide modified flat ceramic membrane. Background Art
[0002] Pharmaceutical and personal care products are an important class of pharmaceutical chemicals and are widely used around the world. However, due to improper disposal of wastewater generated in the production process of pharmaceutical chemicals by manufacturers and the failure of drugs to be fully absorbed during use, a large portion of them eventually enter natural water bodies in the form of original drugs or metabolites. Although their concentrations in water bodies are low, they have strong endocrine disrupting and genetic toxicity, which may cause bacteria to develop drug resistance, affect the human reproductive system, and have risks of carcinogenic, teratogenic and mutagenic effects.
[0003] Membrane separation technology has attracted much attention in the field of water purification due to its high efficiency, energy saving, easy operation and environmental friendliness. However, the problem of membrane fouling during long-term operation has always been the main obstacle restricting its practical application. At the same time, a single membrane process is limited to the separation function, and the treatment of the concentrated liquid with high concentrations of pollutants produced in the process is also an urgent problem to be solved. In recent years, the combination of advanced oxidation technology and membrane separation technology to prepare catalytic modified membranes has developed into an effective way to solve the above problems.
[0004] Common membrane materials on the market are divided into polymer membranes and ceramic membranes. Ceramic membranes have good chemical stability, which can reduce the damage to the membrane substrate caused by strong oxidizing free radicals generated during the catalytic reaction. In addition, the excellent thermal stability of ceramic membranes makes them more suitable for surface modification by high-temperature sintering methods to achieve stable loading of catalysts.
[0005] At present, many researchers have tried to couple ceramic membranes with advanced oxidation processes to improve membrane performance. For example, a CoFe2O4 catalytic layer is generated in situ on the surface of a ceramic membrane by a hydrothermal method, potassium permonosulfate (PMS) is efficiently activated, and ofloxacin in water is degraded; a ZnO catalytic layer is formed on the surface of a nanoporous ceramic membrane by atomic deposition, which significantly improves the membrane's anti-biofouling ability under UV-A light irradiation; a ceramic membrane with a Ce and Mn oxide coating can catalyze ozone oxidation to degrade persistent organic pollutants in water. However, the above modification methods all form a catalytic layer on the membrane surface, which usually causes the surface membrane pores to be blocked, the water flux drops sharply, and the catalytic reaction only occurs in the catalytic layer, which has a poor degradation effect on small molecular pollutants that cannot be retained by the surface. Summary of the invention
[0006] The purpose of the present invention is to provide a preparation method and application of a nano transition metal oxide modified flat ceramic membrane, which integrates nano-scale transition metal oxides on the surface of ceramic particles inside the flat ceramic membrane through a complexing agent-assisted impregnation-calcination method. The integrated flat ceramic membrane can activate permonosulfate, so it can be used for catalytic degradation of antibiotics such as carbamazepine in water, and it has good anti-pollution ability.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] A nano transition metal oxide modified flat ceramic membrane adopts a complexing agent-assisted impregnation-calcination method to uniformly grow nano-scale transition metal oxides on the surface of ceramic particles inside the flat ceramic membrane to form a catalytic membrane capable of activating permonosulfate.
[0009] The method for preparing the nano transition metal oxide modified flat ceramic membrane comprises the following steps:
[0010] 1) Transition metal complex solution
[0011] The transition metal nitrate and β-cyclodextrin as a complexing agent are dissolved in the same volume of deionized water to prepare a transition metal salt solution and a β-cyclodextrin solution; then, the obtained transition metal salt solution is added to the β-cyclodextrin solution at 40-70°C with stirring, stirred for 1-2 hours, and then aged at room temperature for 4-6 hours to obtain a uniform and stable transition metal complexing solution;
[0012] 2) Transition metal complex solution infiltrates flat ceramic membrane
[0013] After soaking the flat ceramic membrane in the transition metal complex solution for 20-30 min, the transition metal complex solution was vacuum filtered through the flat ceramic membrane at 0.2 MPa for 1-2 times, each time for 30 min, and then the filtered flat ceramic membrane was dried at 80-90 °C for 2-3 h;
[0014] 3) Low temperature calcination
[0015] The dried flat ceramic membrane is placed in a muffle furnace for low-temperature calcination, and after it is naturally cooled to room temperature, a transition metal oxide-modified flat ceramic membrane is obtained.
[0016] Furthermore, the molar ratio of the transition metal nitrate used in step 1) to β-cyclodextrin is 1:1; the transition metal nitrate is cobalt nitrate, copper nitrate, nickel nitrate, zinc nitrate, manganese nitrate or iron nitrate.
[0017] Furthermore, in step 3), the low temperature calcination is carried out by heating from room temperature to 300-500°C at a rate of 2°C / min and keeping the temperature for 120-140min.
[0018] The above-mentioned nano-transition metal oxide modified flat ceramic membrane has a high anti-pollution ability in wastewater containing macromolecular pollutants such as humic acid, and it can achieve the degradation of medicines and personal care products containing antibiotics such as carbamazepine in the presence of persulfate. Therefore, it can be used for the degradation treatment of medicines and personal care products in wastewater containing macromolecular pollutants, and it can still maintain a high water flux after long-term treatment.
[0019] The significant advantages of the present invention are:
[0020] (1) The present invention utilizes a complexing agent-assisted method to uniformly grow transition metal oxide particles on the surface of ceramic particles inside a ceramic membrane, wherein the addition of β-cyclodextrin can effectively inhibit the agglomeration of particles, making the particle size of the resulting transition metal oxide much smaller than the pores inside the membrane, and thus can grow on the surface of ceramic particles inside the ceramic membrane, which can also maintain the original water flux of the ceramic membrane to the greatest extent.
[0021] (2) The present invention firmly fixes nano transition metal oxides on the surface of ceramic particles by calcination, and chemical bonds are formed between the transition metal oxides and alumina, so that the transition metal oxides can be stably present in the ceramic membrane and are not easily lost. In actual applications, the amount of metal ion leaching is extremely low, so the catalytic performance of the resulting ceramic membrane can be stable and long-lasting.
[0022] (3) The present invention uniformly grows nano-transition metal oxides on the surface of ceramic particles inside the ceramic membrane, so that the entire ceramic membrane becomes a reactor. Therefore, the catalytic degradation reaction is not limited to the membrane surface, which allows large molecular pollutants such as humic acid to be retained by the membrane pores, while small-sized pollutants that cannot be retained by the membrane can also be effectively removed when passing through the pores inside the membrane. The membrane pores inside the ceramic membrane act as a microreactor, which can accelerate mass transfer, thereby greatly improving the catalytic performance of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Surface macroscopic comparison diagrams of the initial flat ceramic membrane (a), the flat ceramic membrane after impregnation in Example 1 (b), and the modified flat ceramic membrane (c).
[0024] Figure 2 SEM images of the cross sections of the initial flat ceramic membrane (a, c) and the modified flat ceramic membrane in Example 1 (b, d), respectively.
[0025] Figure 3This is the full XPS spectrum of the cross section of the initial flat ceramic membrane and the modified flat ceramic membrane in Example 1.
[0026] Figure 4 This is a high-resolution Co 2p image of the cross section of the modified flat ceramic membrane in Example 1.
[0027] Figure 5 This is a flow chart of dead-end membrane filtration in Example 2.
[0028] Figure 6 This is a comparison chart of the removal efficiency of CBZ by the flat ceramic membrane modified with nano-Co3O4 under different driving pressures in Example 3.
[0029] Figure 7 This is a cyclic test diagram of the catalytic degradation of CBZ by the flat ceramic membrane modified with nano-Co3O4 in Example 4.
[0030] Figure 8 This is a comparison chart of the membrane flux changes of the initial flat ceramic membrane in Example 5 and the integrated flat ceramic membrane in Example 1 in treating a simulated solution containing humic acid under the joint action of PMS.
[0031] Fig. 9 The figure shows the flux comparison between the flat ceramic membrane with Co3O4 directly loaded on the surface and the flat ceramic membrane modified with nano-Co3O4 in Example 6, as well as the effect comparison of removing carbamazepine in the presence of humic acid. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings. The embodiments described are only some embodiments of the present invention, but not all embodiments.
[0033] Example 1
[0034] The preparation of nano-Co3O4 modified flat composite ceramic membrane specifically includes the following steps:
[0035] 1) Weigh 15 mmol of cobalt nitrate and 15 mmol of β-cyclodextrin respectively, dissolve each in 50 mL of deionized water, add the obtained cobalt nitrate solution dropwise into the obtained β-cyclodextrin under stirring at 60 °C, stir for 1 hour, and place it for aging for 4 hours after the temperature drops to room temperature to obtain a cobalt complex solution;
[0036] 2) The flat ceramic membrane (diameter 47 mm, thickness 2 mm, pore size 100 nm) was immersed in the cobalt complex solution for 30 min, and then the cobalt complex solution was filtered twice by the flat ceramic membrane at 0.2 MPa for 30 min each time, so that the cobalt complex solution could be more fully infiltrated into the ceramic membrane, and then the immersed flat ceramic membrane was placed in a 90 °C oven for 2 h for drying;
[0037] 3) Take out the dried flat ceramic membrane carrier, place it in a muffle furnace, heat it to 300 °C at a rate of 2 °C / min, keep it warm for 120 min, cool it naturally to room temperature and then take it out to obtain a nano-Co3O4 modified flat ceramic membrane.
[0038] Figure 1 The surface macroscopic comparison pictures of the initial flat ceramic membrane (a), the impregnated flat ceramic membrane (b) and the modified flat ceramic membrane (c) are shown. As can be seen from the picture, the initial ceramic membrane is white, which turns pink after being impregnated and dried with cobalt complex, and then turns blue-black after low-temperature calcination.
[0039] Figure 2 The SEM images of the cross sections of the initial flat ceramic membrane (a, c) and the modified flat ceramic membrane (b, d) are shown in Figure 1. From the comparison of the low-magnification SEM images (a, b), it can be seen that in the internal pores of the modified flat ceramic membrane, small particles grow evenly on the surface of the internal ceramic particles. Further comparison of the high-magnification SEM images (c, d) shows that the particles integrated on the surface of the ceramic particles are very small and have not agglomerated, so they will not cause blockage of the membrane pores.
[0040] Figure 3 The full XPS spectra of the cross section of the initial flat ceramic membrane and the modified flat ceramic membrane are shown in the figure. It can be found that the peaks of O and Al in the initial flat ceramic membrane and the modified flat ceramic membrane are very strong, indicating that the main components of the initial flat ceramic membrane and the modified flat ceramic membrane are Al2O3. Through further comparison, it is found that the modified flat ceramic membrane has peaks at 780.1 and 795.5 eV, which are the characteristic peaks corresponding to Co 2p, indicating that the flat ceramic membrane contains cobalt.
[0041] Figure 4 This is a high-resolution spectrum of Co 2p on the cross section of the modified flat ceramic membrane. Analysis of the spectrum shows that the two characteristic peaks at 780.1 and 795.5 eV correspond to Co 2p 1 / 2 and Co 2p 3 / 2 The spin-orbit peaks are respectively related to Co 2+ 781.1, 797.3 eV and Co 3+The peaks at 779.9 eV and 794.3 eV fit very well; and the two fitted peaks at 786.6 and 803.4 eV are their corresponding satellite peaks, which indicates that the particulate material integrated on the ceramic carrier is Co3O4.
[0042] Example 2
[0043] The initial flat ceramic membrane and the nano-Co3O4 modified flat ceramic membrane obtained in Example 1 were placed in Figure 5 In the dead-end filtration system, a simulated solution containing 10 mg / L CBZ and 1.0 mol / L permonosulfate (2KHSO5·KHSO4·K2SO4) was continuously filtered at 0.2 MPa, and the time used to collect 5 mL of pure water at the permeation end was recorded. Each membrane was tested three times and the average value was taken as the pure water membrane flux of the test membrane. The results are shown in Table 1.
[0044] Table 1
[0045]
[0046] As can be seen from Table 1, the porosity of the modified flat ceramic membrane is almost unchanged from that of the flat ceramic membrane, and the water flux is also equivalent, which further proves that the modification method of the present invention does not cause clogging of the membrane pores.
[0047] Example 3
[0048] The nano-Co3O4 modified flat ceramic membrane obtained in Example 1 was placed in Figure 5 In a dead-end filtration system, a simulated solution containing 10 mg / L carbamazepine (CBZ) and 1.0 mM permonosulfate (2KHSO5·KHSO4·K2SO4) was continuously filtered under different pressures (0.05 MPa, 0.10 MPa, 0.20 MPa, and 0.40 MPa). Then, effluent samples (0.5 mL) were collected at the permeation end at certain time intervals, mixed with an equal amount of methanol, and sent to a high-performance liquid chromatography to detect the CBZ concentration in order to evaluate the performance of catalytic membrane activated PMS in degrading CBZ. The results are shown in FIG. Figure 6 shown.
[0049] Driven by different pressures, the water flux of the modified flat ceramic membrane is different (the water flux corresponding to 0.05 MPa, 0.10 MPa, 0.20 MPa and 0.40 MPa is 16 LMH, 34 LMH, 56 LMH and 100 LMH respectively). The difference in flux will cause the time for the permeate to flow through the ceramic membrane to differ, that is, the greater the flux, the shorter the time for the catalyst to activate PMS, the fewer active free radicals are generated and the shorter the time for them to interact with pollutants, so the removal effect of pollutants in the permeate becomes worse. Figure 6It can be seen that the removal rate of CBZ in the first outlet water point obtained by filtration of the modified flat ceramic membrane under different fluxes all reached the optimal value. When the flux is 100 LMH, the removal rate of CBZ at the first outlet water point can reach 68%. When the flux is 16 LMH, the removal rate of carbamazepine at the first outlet water point can reach 91%. This shows that under appropriate membrane flux, the modified flat ceramic membrane has the ability to efficiently remove carbamazepine.
[0050] Example 4
[0051] At 0.2 MPa, a cyclic test of removing CBZ was carried out using the nano-Co3O4 modified flat ceramic membrane activated PMS obtained in Example 1. One cycle was 60 minutes, and the cycle was repeated 5 times. Samples (0.5 mL) were taken at intervals of 10 minutes each time, mixed with an equal amount of methanol, and then sent to a high performance liquid chromatography to detect the CBZ concentration. The results are as follows: Figure 7 shown.
[0052] Depend on Figure 7 It can be seen that the removal efficiency of CBZ was 89% in the first cycle. After 4 cycles, the removal efficiency of CBZ slowly decreased to 88.7%, 87.5%, 86.6% and 85.8%, respectively, and still remained above 85%, indicating that the Co3O4 modified flat ceramic membrane / PMS system has good stability and reusability in removing CBZ.
[0053] Example 5
[0054] The initial flat ceramic membrane and the nano-Co3O4 modified flat ceramic membrane obtained in Example 1 were placed in Figure 5 In the dead-end filtration system, at 0.20 MPa, simulated solutions containing 10 mg / L humic acid and 1.0 mM permonosulfate (2KHSO5·KHSO4·K2SO4) were filtered respectively, and the water flux changes were tested at certain intervals. The results are as follows: Figure 8 shown.
[0055] Depend on Figure 8 It can be seen that using the initial flat ceramic membrane / PMS system, after running for 60 min, the permeation flux of the membrane increased from 34.56 L·m -2 ·h -1 Rapidly dropped to 17.96 L·m -2 ·h -1 This is because humic acid is intercepted by the initial ceramic membrane and continuously accumulates on the membrane surface, causing serious membrane surface contamination and a flux loss of 50%. However, the water flux of humic acid filtered by the modified flat ceramic membrane / PMS system is only 34.46 L·m -2 ·h -1 Down to 31.87 L·m -2·h -1 , the flux loss was only 7.5%. These results show that with the assistance of PMS, the membrane fouling of the modified flat ceramic membrane can be well alleviated, which may be because the active oxidative species generated by Co3O4 activating PMS on the ceramic membrane timely oxidized the macromolecular humic acid retained by the membrane.
[0056] Example 6
[0057] The preparation of the flat composite ceramic membrane with Co3O4 loaded on the surface specifically includes the following steps:
[0058] 1) Weigh 15 mmol of cobalt nitrate and 15 mmol of β-cyclodextrin respectively, dissolve each in 50 mL of deionized water, add the obtained cobalt nitrate solution dropwise to the obtained β-cyclodextrin under stirring at 60 °C, stir for 1 hour, and place it for aging for 4 hours after the temperature drops to room temperature to obtain a cobalt complex solution, which is then evaporated to dryness and placed in a muffle furnace, heated to 300 °C at a rate of 2 °C / min, kept warm for 120 min, cooled naturally to room temperature and taken out to obtain powdered Co3O4;
[0059] 2) The obtained powdered Co3O4 was added to 100 mL of anhydrous ethanol containing 3% bis-[3-(triethoxysilyl)propyl]-tetrasulfide, and ultrasonicated for 20 min. Then, the Co3O4-containing suspension solution was filtered using a flat ceramic membrane (diameter 47 mm, thickness 2 mm, pore size 100 nm) at 0.2 MPa, and then placed in a 90 °C oven for 2 h to obtain a flat composite ceramic membrane with Co3O4 loaded on the surface.
[0060] The obtained surface-loaded Co3O4 flat composite ceramic membrane and the nano-Co3O4 modified flat ceramic membrane obtained in Example 1 were jointly subjected to flux testing; then the two were used to degrade the simulated pollutant carbamazepine under the operating conditions of 50 mg / L humic acid and 1.0 mM permonosulfate (2KHSO5·KHSO4·K2SO4). The results are shown in FIG. Fig. 9 shown.
[0061] Depend on Fig. 9 It can be seen that the flux of the ceramic membrane directly loaded with Co3O4 increased from the initial 34.56 L·m -2 ·h -1 Reduced to 25.16L·m -2 ·h -1, indicating that there is membrane clogging. At the same time, under the influence of humic acid, the ceramic membrane with direct surface loading of Co3O4 has only 53% degradation effect on carbamazepine. This is because the Co3O4 on the membrane surface lacks the protection of the membrane. Under long-term exposure to water environment conditions, macromolecular humic acid will adhere to the Co3O4 surface, resulting in a reduction in active sites and a poor catalytic effect. The Co3O4-modified flat ceramic membrane, because the Co3O4 inside the membrane pores is protected by the surface pore size effect, still has efficient removal performance for carbamazepine under the interference of humic acid, and its removal capacity is comparable to that without humic acid interference. It is thus explained that the present invention integrates transition metal oxides in the ceramic membrane matrix, which can not only maintain the flux of the membrane to a large extent, but also has a strong ability to resist interference from macromolecular pollutants.
[0062] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. Application of a nano transition metal oxide modified flat ceramic membrane in catalytic degradation of carbamazepine in water, characterized in that: In the presence of peroxymonosulfate, the nano transition metal oxide modified flat ceramic membrane can be used for the degradation treatment of carbamazepine in wastewater; The preparation method of the nano transition metal oxide modified flat ceramic membrane comprises the following steps: 1) Weigh 15 mmol of cobalt nitrate and 15 mmol of β-cyclodextrin respectively, dissolve each in 50 mL of deionized water, add the obtained cobalt nitrate solution dropwise into the obtained β-cyclodextrin under stirring at 60°C, stir for 1 hour, and place it for aging for 4 hours after the temperature drops to room temperature to obtain a cobalt complex solution; 2) A flat ceramic membrane with a diameter of 47 mm, a thickness of 2 mm, and a pore size of 100 nm was immersed in the cobalt complex solution for 30 min, and then a vacuum filtration device was used to filter the cobalt complex solution twice at 0.2 MPa, each time for 30 min, so that the cobalt complex solution could be more fully infiltrated into the ceramic membrane, and then the immersed flat ceramic membrane was placed in a 90 °C oven for 2 h for drying; 3) Take out the dried flat ceramic membrane carrier, place it in a muffle furnace, heat it to 300°C at a rate of 2°C / min, keep it warm for 120 min, cool it naturally to room temperature and then take it out to obtain a nano-Co3O4 modified flat ceramic membrane.