Preparation method of cellulose / seaweed polysaccharide flame retardant composite material
By cross-linking cellulose nanofibers with seaweed polysaccharide and calcium ions, a stable cellulose/seaweed polysaccharide flame retardant composite material is prepared, which solves the problems of flammability of plant fibers and the harm of traditional flame retardants, and achieves high efficiency and environmental protection. , degradable flame retardant effect.
Patent Information
- Application Number
- CN202310328882.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Existing plant fiber materials are flammable and the added flame retardants are harmful to the human body and the environment, and are non-degradable.
By cross-linking cellulose nanofibers with seaweed polysaccharide and calcium ions to form covalent bonds, a stable cellulose/seaweed polysaccharide flame-retardant composite material is prepared, using etching, oxidation treatment and hot pressing methods to form a non-toxic, environmentally friendly, Flame retardant multifunctional composite material.
It achieves the high-efficiency flame retardant effect of plant fibers, and at the same time the material is degradable, avoiding the harm of traditional flame retardants to the human body and the environment, and the preparation method is simple and highly practical.
Smart Images

Figure CN116285010B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flame retardant composite materials, and in particular relates to a method for preparing a cellulose / seaweed polysaccharide flame retardant composite material. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Cellulose is a macromolecular polysaccharide composed of glucose. It is the most widely distributed and abundant polysaccharide in nature. Cellulose has great application prospects in the field of composite materials (especially medical fibers, commercial paper, etc.). How to prepare multifunctional cellulose composite materials has attracted widespread attention from all walks of life.
[0004] Plant fibers are flammable. Currently, in the plant fiber market, flame retardants are mainly added to prevent fires. However, some flame retardants are easily harmful to the human body. For example, brominated flame retardants are easily accumulated in the human body, which will interfere with the endocrine, immune and nervous systems of the human body; halogen-containing flame retardants will produce a lot of smoke and toxic gases when burning, which is very harmful to the human body; phosphorus-containing flame retardants are highly volatile, have poor heat resistance, and produce dripping when burning. In addition, composite materials with flame retardants are non-degradable and easily cause harm to the environment. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a method for preparing a cellulose / seaweed polysaccharide flame retardant composite material. The cellulose / seaweed polysaccharide flame retardant composite material prepared in the present application forms a stable network structure by cross-linking cellulose nanofibers and seaweed polysaccharides with calcium ions to produce covalent bonds. In addition, the method has a wide source of raw materials, a simple preparation method, and is environmentally friendly.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The first aspect of the present invention provides a method for preparing a cellulose / seaweed polysaccharide flame retardant composite material, comprising:
[0008] The plant fibers are etched and oxidized to obtain cellulose nanofibers;
[0009] The seaweed polysaccharide aqueous solution is mixed with the cellulose nanofibers and hot-pressed to obtain a cellulose nanofiber / seaweed polysaccharide composite material;
[0010] Spraying a solution containing calcium ions on the cellulose nanofiber / seaweed polysaccharide composite material, and air-drying the mixture to obtain a cellulose / seaweed polysaccharide flame retardant composite material;
[0011] The mass concentration of the seaweed polysaccharide aqueous solution is 1.0% to 2.0%;
[0012] The usage ratio of cellulose nanofibers to seaweed polysaccharides is 10:1-1.5.
[0013] The invention develops a multifunctional cellulose composite material with the characteristics of being non-toxic, flame-retardant and environmentally friendly, which is of great significance for developing the plant fiber market.
[0014] The second aspect of the present invention provides a cellulose / seaweed polysaccharide flame retardant composite material prepared by the above method.
[0015] The third aspect of the present invention provides the use of the above-mentioned cellulose / seaweed polysaccharide flame retardant composite material in the preparation of flame retardant materials.
[0016] Beneficial Effects of the Invention
[0017] (1) The present application provides a method for preparing a cellulose / seaweed polysaccharide flame-retardant composite material, wherein plant fibers are etched and oxidized to quickly prepare cellulose nanofibers. Such cellulose nanofibers not only retain the original characteristics of the plant fibers, but also change the molecular structure and improve the strength of the fibers. Divalent metal ions are cross-linked with cellulose nanofibers and seaweed polysaccharides to form covalent bonds, thereby forming a stable cross-linked network. Compared with the method of introducing metal ions into cellulose fibers using a cosolvent, the method has higher efficiency and success rate, making it possible for the method to be used in more applications in the field of composite materials.
[0018] (2) The preparation method of the present invention is simple, practical and easy to promote. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention, and the exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute improper limitations on the present invention.
[0020] Figure 1 This is a scanning electron microscope photograph of the cellulose / seaweed polysaccharide flame retardant composite material prepared in Example 1 of the present invention.
[0021] Figure 2 This is a scanning electron microscope photograph of the cellulose / seaweed polysaccharide flame retardant composite material prepared in Example 2 of the present invention.
[0022] Figure 3 This is a scanning electron microscope photograph of the cellulose flame retardant material prepared in Comparative Example 1 of the present invention.
[0023] Figure 4 This is a scanning electron microscope photograph of the cellulose flame retardant material prepared in Comparative Example 2 of the present invention.
[0024] Figure 5 These are stress-strain curves of the cellulose / seaweed polysaccharide flame retardant composite materials and cellulose flame retardant materials prepared in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 of the present invention.
[0025] Figure 6 The infrared spectra of the cellulose / seaweed polysaccharide flame retardant composite materials and cellulose flame retardant materials prepared in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 of the present invention are shown.
[0026] Figure 7 The thermogravimetric diagrams of the cellulose / seaweed polysaccharide flame retardant composite materials and the cellulose flame retardant materials prepared in Example 1, Example 2, Comparative Example 1 and Comparative Example 2 of the present invention under air atmosphere. DETAILED DESCRIPTION
[0027] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0028] A method for preparing a cellulose / seaweed polysaccharide flame-retardant composite material will not cause rapid degradation of seaweed polysaccharide in a strong alkaline solution of cellulose and loss of raw materials, has the advantages of high success rate, flame retardancy, high toughness, and biodegradability, and can be degraded into carbon dioxide and water under certain conditions to achieve renewable utilization of resources.
[0029] The following steps are involved:
[0030] 1) Prepare wood powder from which lignin and hemicellulose are removed by kraft pulping;
[0031] 2) oxidizing the wood powder in step 1) by TEMPO oxidation to obtain cellulose nanofibers;
[0032] 3) adding the cellulose nanofibers from step 2) into the algae polysaccharide aqueous solution, mixing, and hot pressing to obtain a cellulose nanofiber / algae polysaccharide composite material;
[0033] 4) spraying the aqueous solution containing calcium ions on the composite material prepared in step 3) to react and obtain a cellulose / seaweed polysaccharide flame retardant composite material;
[0034] In some embodiments, the poplar wood powder has a particle size of 300-400 meshes, and the sulfate method is: at a temperature of 80-100° C., the poplar wood powder is immersed in a mixed solution of 4.0%-5.0% sodium hydroxide and 2.5%-3.0% sodium sulfite.
[0035] In some embodiments, the TEMPO oxidation method is as follows: at a temperature of 30 to 40° C., the wood powder from which lignin and hemicellulose have been removed is placed in a mixed solution of 0.1 mM TEMPO oxidant, 1.0% sodium chlorite and 1.0% sodium hypochlorite and stirred for 6 to 24 hours.
[0036] In some embodiments, the mass concentration of the seaweed polysaccharide solution is 1.0% to 2.0%.
[0037] In some embodiments, the ratio of cellulose nanofibers to seaweed polysaccharide powder in the mixed solution is 10:1-1.5.
[0038] In some embodiments, the reaction is a cross-linking reaction between calcium ions and seaweed polysaccharides and cellulose nanofibers.
[0039] In some embodiments, the hot pressing pressure is 20-100 MPa, the heating temperature is 80-90° C., and the hot pressing time is 25-30 min.
[0040] In some embodiments, the aqueous solution containing calcium ions is an aqueous solution of calcium chloride with a mass concentration of 3% to 5%.
[0041] In some embodiments, 10 to 30 ml of calcium chloride aqueous solution is sprayed on the prepared composite material and allowed to air dry naturally at room temperature.
[0042] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are intended to explain the present invention rather than to limit it.
[0043] Example 1
[0044] Step 1: Removal of lignin and hemicellulose
[0045] The poplar wood powder was immersed in 1000 ml of a mixed aqueous solution of 4.0% sodium hydroxide and 2.5% sodium sulfite, and boiled in boiling water for 6 hours. After the heating was completed, the boiled wood powder was repeatedly rinsed with deionized water to obtain wood powder with lignin and hemicellulose removed.
[0046] Step 2: Preparation of oxidizing reagent
[0047] A mixed aqueous solution of 0.1 mM TEMPO oxidant and 1.0% sodium chlorite was prepared and dissolved at 30° C. for 1 h.
[0048] Step 3: Oxidation of cellulose fibers
[0049] Add a 1.0% sodium hypochlorite aqueous solution and the wood powder obtained in step 1 to the mixed solution obtained in step 2. Stir the suspension at 2000 r / min and 35° C. for 6 hours. After cooling the suspension to room temperature, wash the remaining chemicals on the surface with deionized water to obtain oxidized cellulose fibers.
[0050] Step 4: Preparation of cellulose nanofibers
[0051] The oxidized cellulose fibers obtained in step 3 were cut into cellulose nanofibers at high speed using a fiber standard disintegrator at a rotation speed of 50,000 rpm for 2 minutes to obtain cellulose nanofibers.
[0052] Step 5: Prepare cellulose nanofiber / seaweed polysaccharide mixed solution
[0053] A 1.0% seaweed polysaccharide solution was prepared at room temperature using a high-speed stirrer, cellulose nanofibers were added to the solution, and a mixed solution with a mass ratio of cellulose nanofibers to seaweed polysaccharide powder of 10:1 was prepared using a stirrer.
[0054] Step 6: Preparation of cellulose nanofiber / seaweed polysaccharide composite profiles
[0055] The mixed solution obtained in step five was placed in a mold, and hot-pressed on a hot press at a temperature of 90° C. and a pressure of 100 MPa for 30 minutes to prepare a cellulose nanofiber / seaweed polysaccharide composite material.
[0056] Step 7: Preparation of cellulose / seaweed polysaccharide flame retardant composite material
[0057] Spray 20 ml of 3% calcium chloride aqueous solution on the cellulose nanofiber / seaweed polysaccharide composite profile in step 6, and air dry it at room temperature to obtain a cellulose / seaweed polysaccharide flame retardant composite material. After testing, the LOI of the cellulose / seaweed polysaccharide flame retardant composite material is 32%. Figure 1 As shown, the surface of the cellulose / seaweed polysaccharide flame retardant composite material shows cellulose nanofibers, such as Figure 5 As shown in FIG. 1 , the tensile strength of the cellulose / seaweed polysaccharide flame retardant composite material is 57.2 Mpa. Figure 6 Shown at 1560~1610cm -1 The absorption peak at is the stretching vibration peak of carboxylate, indicating that calcium ions react with cellulose nanofibers and seaweed polysaccharides to form a cross-linking reaction, such as Figure 7 The residual carbon content of the cellulose / seaweed polysaccharide flame retardant composite material at 600° C. is 20%.
[0058] Example 2
[0059] Step 1: Removal of lignin and hemicellulose
[0060] The poplar wood powder was immersed in 1000 ml of a mixed aqueous solution of 4.0% sodium hydroxide and 2.5% sodium sulfite, and boiled in boiling water for 6 hours. After the heating was completed, the boiled wood powder was repeatedly rinsed with deionized water to obtain wood powder with lignin and hemicellulose removed.
[0061] Step 2: Preparation of oxidizing reagent
[0062] A mixed aqueous solution of 0.1 mM TEMPO oxidant and 1.0% sodium chlorite was prepared and dissolved at 30° C. for 1 h.
[0063] Step 3: Oxidation of cellulose fibers
[0064] Add 1.0% sodium hypochlorite solution and the wood powder obtained in step 1 to the mixed solution obtained in step 2. Stir the suspension at 2000 r / min and 35° C. for 6 hours. After cooling the suspension to room temperature, wash the remaining chemicals on the surface with deionized water to obtain oxidized cellulose fibers.
[0065] Step 4: Preparation of cellulose nanofibers
[0066] The oxidized cellulose fibers obtained in step 3 were cut into cellulose nanofibers at high speed for 2 minutes using a fiber standard disintegrator at a rotation speed of 50,000 rpm to obtain cellulose nanofibers.
[0067] Step 5: Prepare cellulose nanofiber / seaweed polysaccharide mixed solution
[0068] A 1.0% seaweed polysaccharide solution was prepared at room temperature using a high-speed stirrer, cellulose nanofibers were added to the solution, and a mixed solution with a mass ratio of cellulose nanofibers to seaweed polysaccharide powder of 10:1 was prepared using a stirrer.
[0069] Step 6: Preparation of cellulose nanofiber / seaweed polysaccharide composite film
[0070] The mixed solution obtained in step five is placed in a paper sheet former for filtration, and the filtered cellulose / seaweed polysaccharide composite material is heated on a volt-pressure weight at a temperature of 90° C. and a pressure of 20 MPa for 30 minutes to prepare a cellulose nanofiber / seaweed polysaccharide composite film.
[0071] Step 7: Preparation of cellulose / seaweed polysaccharide flame retardant composite material
[0072] Spray 10 ml of 3% calcium chloride aqueous solution on the cellulose / seaweed polysaccharide flame retardant composite film in step 6, and air dry it at room temperature to obtain a cellulose / seaweed polysaccharide flame retardant composite material. After testing, the LOI of the cellulose / seaweed polysaccharide flame retardant composite material is 30%. Figure 2 As shown, the surface of the cellulose / seaweed polysaccharide flame retardant composite material shows cellulose nanofibers, such as Figure 5 As shown in FIG. 1 , the tensile strength of the cellulose / seaweed polysaccharide flame retardant composite material is 22.8 MPa. Figure 6 The cellulose / seaweed polysaccharide flame retardant composite material has a thermal conductivity of 1560-1610 cm -1 The absorption peak at is the stretching vibration peak of carboxylate, indicating that calcium ions react with cellulose nanofibers and seaweed polysaccharides to form a cross-linking reaction, such as Figure 7 The residual carbon content of the cellulose / seaweed polysaccharide flame retardant composite material at 600°C is 16%.
[0073] Comparative Example 1
[0074] Step 1: Removal of lignin and hemicellulose
[0075] The poplar wood powder was immersed in 1000 ml of a mixed aqueous solution of 4.0% sodium hydroxide and 2.5% sodium sulfite, and boiled in boiling water for 6 hours. After the heating was completed, the boiled wood powder was repeatedly rinsed with deionized water to obtain wood powder with lignin and hemicellulose removed.
[0076] Step 2: Preparation of oxidizing reagent
[0077] A mixed aqueous solution of 0.1 mM TEMPO oxidant and 1.0% sodium chlorite was prepared and dissolved at 30° C. for 1 h.
[0078] Step 3: Oxidation of cellulose fibers
[0079] Add a 1.0% sodium hypochlorite aqueous solution and the wood powder obtained in step 1 to the mixed solution obtained in step 2. Stir the suspension at 2000 r / min and 35° C. for 6 hours. After cooling the suspension to room temperature, wash the remaining chemicals on the surface with deionized water to obtain oxidized cellulose fibers.
[0080] Step 4: Preparation of cellulose nanofibers
[0081] The oxidized cellulose fibers obtained in step 3 were cut into cellulose nanofibers at high speed using a fiber standard disintegrator at a rotation speed of 50,000 rpm for 2 minutes to obtain cellulose nanofibers.
[0082] Step 5: Preparation of cellulose nanofiber profiles
[0083] The cellulose nanofibers obtained in step 4 were placed in a mold and hot-pressed on a hot press at a temperature of 90° C. and a pressure of 100 MPa for 30 minutes to prepare a cellulose nanofiber profile.
[0084] Step 6: Preparation of cellulose flame retardant material
[0085] Spray 20 ml of 3% calcium chloride aqueous solution on the cellulose nanofiber profile in step 5, and air dry it at room temperature to obtain a cellulose flame retardant material. Figure 3 As shown in FIG. 5 , the surface of the cellulose flame retardant material shows cellulose nanofibers. As shown in FIG. 5 , the tensile strength of the cellulose flame retardant material is 36.7 Mpa. Figure 6 The absorption peaks at 1560-1610 cm-1 are the stretching vibration peaks of carboxylates, indicating the cross-linking reaction between calcium ions and cellulose nanofibers, such as Figure 7 The residual carbon content of the cellulose / seaweed polysaccharide flame retardant composite material at 600°C is 12%.
[0086] Comparative Example 2
[0087] Step 1: Removal of lignin and hemicellulose
[0088] The poplar wood powder was immersed in 1000 ml of a mixed aqueous solution of 4.0% sodium hydroxide and 2.5% sodium sulfite, and boiled in boiling water for 6 hours. After the heating was completed, the boiled wood powder was repeatedly rinsed with deionized water to obtain wood powder with lignin and hemicellulose removed.
[0089] Step 2: Preparation of oxidizing reagent
[0090] A mixed aqueous solution of 0.1 mM TEMPO oxidant and 1.0% sodium chlorite was prepared and dissolved at 30° C. for 1 to 2 hours.
[0091] Step 3: Oxidation of cellulose fibers
[0092] Add 1.0% sodium hypochlorite solution and the wood powder obtained in step 1 to the mixed solution obtained in step 2. Stir the suspension at 2000 r / min and 35° C. for 6 hours. After cooling the suspension to room temperature, wash the remaining chemicals on the surface with deionized water to obtain oxidized cellulose fibers.
[0093] Step 4: Preparation of cellulose nanofibers
[0094] The cellulose nanofibers obtained in step 3 were cut at high speed for 2 minutes using a fiber standard disintegrator at a rotation speed of 50,000 rpm to obtain cellulose nanofibers.
[0095] Step 5: Preparation of cellulose flame retardant material
[0096] The cellulose nanofibers in step 4 are placed in 100 ml of 3% calcium chloride aqueous solution, filtered through a paper sheet former, and the filtered cellulose nanofibers are hot-pressed on a 20 MPa weight at 80°C for 30 minutes to obtain a cellulose flame retardant material. Figure 4As shown in FIG. 5 , the surface of the cellulose flame retardant material shows cellulose nanofibers. As shown in FIG. 5 , the tensile strength of the cellulose flame retardant material is 12 Mpa. Figure 6 The absorption peak of the cellulose flame retardant material at 1560-1610 cm-1 is the stretching vibration peak of the carboxylate, indicating that calcium ions and cellulose nanofibers produce a cross-linking reaction, such as Figure 7 The residual carbon content of the cellulose / seaweed polysaccharide flame retardant composite material at 600°C is 2%.
[0097] Experimental Example 1
[0098] The flame retardant properties of natural cellulose and Example 1 and Example 2 were tested, as shown in Table 1:
[0099] Table 1 Comparison of flame retardant data of natural cellulose and Example 1 and Example 2
[0100]
[0101] LOI: limiting oxygen index; pkHRR: heat release rate; THR: total heat release.
[0102] Test conditions:
[0103] Limiting Oxygen Index (LOI) The LOI test was carried out on a HC-2 limiting oxygen index tester according to ISO 4589-1:1996 standard method. The size of all samples was 130 mm × 10 mm.
[0104] The combustion performance pkHRR and THR data were obtained by CONE test: Dual Analysis ConeCalorimeter (FFT, UK) was used according to ISO 5660-1 standard at a heat flux of 35 kW / m 2 Under the conditions of fire, the combustion hazard of materials with sample size of 100mm×100mm×3mm was tested.
[0105] Table 1 is a comparison of flame retardant data of natural cellulose and Example 1 and Example 2. As can be seen from Table 1, the limiting oxygen index of Example 1 and Example 2 exceeds 27%, which is a flame retardant material. In addition, the heat release rate and total heat release of Example 1 and Example 2 are lower than that of natural wood.
[0106] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a cellulose / seaweed polysaccharide flame retardant composite material, It is characterized in that include: The seaweed polysaccharide aqueous solution is mixed with the cellulose nanofibers and hot-pressed to obtain a cellulose nanofiber / seaweed polysaccharide composite material; Spraying a solution containing calcium ions on the cellulose nanofiber / seaweed polysaccharide composite material, and air-drying the mixture to obtain a cellulose / seaweed polysaccharide flame retardant composite material; The mass concentration of seaweed polysaccharide aqueous solution is 1.0%~2.0%; The ratio of cellulose nanofibers to seaweed polysaccharides is 10:1~1.5; The preparation method of the cellulose nanofibers comprises: The kraft pulping method is used to prepare wood powder from which lignin and hemicellulose are removed; The wood powder is oxidized by TEMPO oxidation method to obtain cellulose nanofibers.
2. The method for preparing the cellulose / seaweed polysaccharide flame retardant composite material according to claim 1, It is characterized in that The hot pressing pressure is 20~100Mpa, the heating temperature is 80~90℃, and the hot pressing time is 25~30min.
3. The method for preparing the cellulose / seaweed polysaccharide flame retardant composite material according to claim 1, It is characterized in that The aqueous solution containing calcium ions is a calcium chloride aqueous solution with a mass concentration of 3% to 5%.
4. The method for preparing the cellulose / seaweed polysaccharide flame retardant composite material according to claim 1, It is characterized in that The kraft pulping method comprises the following steps: immersing poplar wood powder in a mixed solution of 4.0% to 5.0% sodium hydroxide and 2.5% to 3.0% sodium sulfite at a temperature of 80 to 100° C. and cooking the mixture.
5. The method for preparing the cellulose / seaweed polysaccharide flame retardant composite material according to claim 1, It is characterized in that The specific conditions of the TEMPO oxidation method are as follows: at a temperature of 30-40° C., the wood powder from which lignin and hemicellulose have been removed is placed in a mixed solution of 0.1-0.15 mM TEMPO oxidant, 1.0%-1.5% sodium chlorite and 1.0%-1.5% sodium hypochlorite and stirred for 6-24 hours.
6. The method for preparing the cellulose / seaweed polysaccharide flame retardant composite material according to claim 1, It is characterized in that The particle size of the wood powder is 300-400 meshes.
7. The method for preparing the cellulose / seaweed polysaccharide flame retardant composite material according to claim 1, It is characterized in that The air drying was performed at room temperature.
8. A cellulose / seaweed polysaccharide flame retardant composite material prepared by the method according to any one of claims 1 to 7.
9. Use of the cellulose / seaweed polysaccharide flame retardant composite material according to claim 8 in the preparation of flame retardant materials.