A method for preparing high-quality pyrolysis oil by catalytic pyrolysis of waste tires based on concentrated solar heat source

Through the combination of concentrated solar pyrolysis technology and carbon-based solid acid catalyst, the efficient recycling and utilization of waste tires, waste sponges and waste leather is solved, and the production of high-quality pyrolysis oil is achieved, reducing carbon emissions and energy consumption. It has also expanded the application fields of waste sponges and waste leather.

CN116286073BActive Publication Date: 2024-11-22GUANGZHOU INST OF ENERGY CONVERSION CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211586990.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-22
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The prior art has problems of waste of resources and greenhouse gas emissions when dealing with organic residues of scrapped vehicles, especially waste tires, waste sponges and waste leather. The traditional pyrolysis method consumes high energy and is accompanied by pollutant emissions.

Method used

The waste tire is catalyzed with concentrated solar heat source, and the waste sponge and waste leather are prepared as biochar and carbon-based solid acid is obtained by acid treatment as a catalyst to improve the yield and quality of the pyrolytic oil.

Benefits of technology

The production of high-quality pyrolytic oil has been achieved, which reduces carbon emissions, reduces the consumption of traditional fossil energy, provides a harmless and resource-based recycling and utilization method, and significantly improves the yield of pyrolytic oil in waste tires and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003990840460000101
    Figure BDA0003990840460000101
Patent Text Reader

Abstract

The invention discloses a method for preparing high-quality pyrolysis oil by catalytic pyrolysis of waste tires based on concentrated solar energy heat source, a synergistic and efficient conversion mode of organic dismantling residues of scrapped vehicles under a new type of heat source, constructs an organic solid waste autocatalytic system, selects different coping methods according to the element composition and physicochemical characteristics of the organic dismantling residues of scrapped vehicles, prepares waste sponges and waste leathers with high content of miscellaneous elements and rich functional groups into biochar, obtains carbon-based solid acid after acid treatment, adopts concentrated solar energy simulated light source as reaction heat source, catalyzes the pyrolysis of waste tire particles, improves the yield and quality of pyrolysis oil, and provides a new, harmless and resource-based way for the recycling and utilization of organic dismantling residues of scrapped vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the technical field of waste treatment, and in particular to a method for preparing high-quality pyrolysis oil by catalytic pyrolysis of waste tires based on a concentrated solar heat source. Background technology:

[0002] At present, people's focus on the recycling of scrapped cars is mainly on its inorganic metal components. However, the organic dismantling parts of scrapped cars (such as waste tires, waste sponges, waste leather, etc.) also have a considerable total amount of recyclables. Therefore, the efficient and clean recycling and upgrading of organic dismantling parts of scrapped cars is also worthy of attention. Waste tires, waste sponges, and waste leather are the three most representative types of organic dismantling parts of automobiles. The C content of waste tires is as high as 80% or more. Improper disposal methods will cause a huge waste of resources and lead to a large amount of greenhouse gas emissions. In contrast, the oxygen content of waste sponges and waste leather is relatively high, and it is difficult to obtain high-quality pyrolysis oil with low oxygen content by pyrolysis alone. In addition, waste leather and waste sponges also contain more impurity elements such as N and S. Therefore, from the perspective of resource recycling, waste leather and waste sponges are not suitable for recycling by pyrolysis.

[0003] Currently, the energy sources of traditional pyrolysis methods are mainly electric heating or fuel combustion heat release. The above methods have high energy consumption and are accompanied by the emission of pollutants. Summary of the invention:

[0004] The purpose of the present invention is to provide a method for preparing high-quality pyrolysis oil by catalytic pyrolysis of waste tires based on concentrated solar heat source. Different coping methods are selected according to the element composition and physicochemical characteristics of organic dismantling residues of scrapped vehicles, waste sponges and waste leathers with high content of miscellaneous elements and rich functional groups are prepared as biochar, and carbon-based solid acid is obtained after acid treatment. Concentrated solar energy simulated light source is used as a reaction heat source to catalyze the pyrolysis of waste tire particles, thereby constructing an organic solid waste self-catalytic system, improving the yield and quality of pyrolysis oil, and providing a new, harmless and resource-based approach for the recycling and utilization of organic dismantling residues of scrapped vehicles.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing high-quality pyrolysis oil by catalytic pyrolysis of waste tires based on concentrated solar heat source, the method comprising the following steps:

[0007] (1) Place scrapped car organic dismantling waste sponge or waste leather particles in a quartz boat and send it into a tube furnace, heat it to 400-800°C at a heating rate of 10°C / min under an inert atmosphere and keep it warm for 1-12 hours to carbonize it. After the reaction is completed, take it out and grind it after it is naturally cooled. Then place it in 1-12wt.% hydrofluoric acid (preferably 9-10wt.%, most preferably 10wt.%), stir it at room temperature for 4-8 hours to remove inorganic components, wash and filter it until the filtrate is neutral, vacuum dry it at 75-85°C for 10-12 hours, then take it out and grind it to obtain biochar;

[0008] (2) Loading the biochar prepared in step (1) with phosphate groups, specifically, the steps are as follows: adding the biochar to deionized water, then adding phosphoric acid, mixing and ultrasonically dispersing for 12 hours, then washing with deionized water and filtering, repeating three times, placing the filter cake in a vacuum drying oven at 75-80° C. and vacuum drying for 12-14 hours, cooling and grinding to obtain a carbon-based solid acid loaded with phosphate groups;

[0009] Alternatively, the biochar prepared in step (1) is loaded with sulfonic acid groups, specifically the following steps: adding the biochar to dichloromethane, then adding chlorosulfonic acid, stirring the reaction at room temperature to 70°C (preferably 60 to 70°C, most preferably 65°C) for 12 hours, then washing with deionized water and filtering, repeating three times, placing the filter cake in a vacuum drying oven at 75-80°C for 12-14 hours, cooling, taking it out and grinding it to obtain a carbon-based solid acid loaded with sulfonic acid groups;

[0010] (3) placing the carbon-based solid acid loaded with phosphoric acid groups or the carbon-based solid acid catalyst loaded with sulfonic acid groups prepared in step (2) and the waste tire particles of scrapped organic demolition residues in a reactor, adjusting the power of the concentrated solar energy simulation light source, heating the reactants at different energy flux densities under an inert atmosphere, discharging the pyrolysis products through the purge gas, and collecting the liquid products after condensation; the mass ratio of the waste tire to the carbon-based solid acid catalyst is 1:0.5-5; the light energy flux density of the concentrated solar energy pyrolysis is 500-1500KW / m 2 The pyrolysis temperature is 400-900°C and the pyrolysis time is 0.5-3h.

[0011] Preferably, in step (2), the mass volume ratio of biochar to phosphoric acid or chlorosulfonic acid is 1 g: (0.1-2) mL.

[0012] Preferably, the particle size of the waste tire particles is 50 to 200 meshes.

[0013] The beneficial effects of the present invention are as follows:

[0014] 1) The present invention utilizes the rich functional groups naturally possessed by waste leather and waste sponge, and carbonizes them to prepare carbon-based solid acid, which is used as a catalyst for the pyrolysis of waste tires. While reducing carbon emissions, the catalytic activity can be improved by relying on the acidic and alkaline sites provided by the rich functional groups. Under the catalytic action of carbon-based solid acid, waste tires can be converted into high-quality pyrolysis oil, which improves the recycling rate of resources from an economic perspective. Carbon-based solid acid raw materials are common and easy to regenerate, and are a low-cost catalyst with good economic benefits.

[0015] 2) The present invention uses concentrated solar energy with high energy density to heat the reactants, which can reduce the consumption of traditional fossil energy, and no additional pollutants are introduced into the entire pyrolysis process. In addition, the light source heating can not only provide the heat required for the reaction, but also stimulate the photocatalytic activity of some catalysts, thereby improving the catalytic effect and obtaining high-yield high-quality pyrolysis oil, which has broad research prospects and practical application value.

[0016] 3) The present invention provides a method for preparing high-quality pyrolysis oil by catalytic pyrolysis of waste tires based on concentrated solar heat sources. The waste tires are heated by simulated solar light sources in an oxygen-free environment, and under the catalytic action of waste sponge / waste leather-derived carbon-based solid acid, efficient conversion of waste tires to high-quality pyrolysis oil is achieved by regulating pyrolysis parameters, which proposes a new method for the pyrolysis of organic residues from scrapped cars and expands the application field of waste sponges and waste leather.

[0017] In summary, the present invention explores a synergistic and efficient conversion method for organic residues from scrapped vehicles under a new type of heat source, constructs an organic solid waste self-catalytic system, selects different coping methods according to the elemental composition and physicochemical properties of organic residues from scrapped vehicles, and prepares waste sponges and waste leathers with rich functional groups and high content of impurities into biochar, obtains carbon-based solid acid after acid treatment, and uses concentrated solar energy simulated light source as a reaction heat source to catalyze the pyrolysis of waste tire particles, thereby improving the yield and quality of pyrolysis oil, providing a new, harmless and resource-based approach for the recycling of organic residues from scrapped vehicles. Specific implementation method:

[0018] The following is a further description of the present invention, rather than a limitation of the present invention.

[0019] Embodiment 1:

[0020] (1) The organic waste leather of scrapped automobiles was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 700°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 6 hours. After the reaction was completed, it was taken out and ground after natural cooling. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL deionized water and 1mL phosphoric acid (H3PO4, AR, 85wt.%) were added to 1g of biochar, and ultrasonic dispersion was performed for 12 hours, followed by washing and filtering. This was repeated three times. The filter cake was vacuum dried at 80°C for 12 hours, and then ground after cooling to obtain a carbon-based solid acid catalyst, which was recorded as 1P-LC6-700.

[0021] (2) 200 mesh automobile waste tire particles and the carbon-based solid acid catalyst prepared in step (1) were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 1300 KW / m 2 The light flux density was used to heat it to 700℃ and maintain it for 2h. After the reaction, the pyrolysis oil obtained by condensation was collected and the yield of pyrolysis oil was 62.1wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 87.9wt.%, as shown in Table 1.

[0022] Comparative Example 1:

[0023] The same as Example 1, except that no carbon-based solid acid catalyst was added during the pyrolysis process, and the final pyrolysis oil yield was 40.7wt.%, and the aromatic content of the pyrolysis oil was 68.6wt.%.

[0024] It can be seen from Example 1 and Comparative Example 1 that the carbon-based solid acid catalyst can significantly improve the yield and quality of waste tire pyrolysis oil under concentrated solar energy heating conditions.

[0025] Embodiment 2:

[0026] (1) The organic waste sponge of scrapped automobiles was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 700°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 6 hours. After the reaction was completed, it was taken out and ground after natural cooling. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL of deionized water and 1mL of phosphoric acid (H3PO4, AR, 85wt.%) were added to 1g of biochar, and after ultrasonic dispersion for 12 hours, the mixture was washed, filtered, and dried to obtain a carbon-based solid acid catalyst 1P-LC6-700.

[0027] (2) 200 mesh automobile waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 1300 KW / m2 The light flux density was used to heat it to 700°C and maintain it for 2 hours. After the reaction, the pyrolysis oil obtained by condensation was collected, and the pyrolysis oil yield was 56.4wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 77.3wt.%, as shown in Table 1.

[0028] Embodiment 3:

[0029] (1) The scrapped car organic dismantling waste leather was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 700°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 6 hours. After the reaction was completed, it was taken out and ground after natural cooling. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL of dichloromethane and 1mL of chlorosulfonic acid (ClHSO3, AR, 99%) were added to 1g of biochar, and the reaction was stirred at 65°C for 12 hours, and then washed, filtered, and dried to obtain a carbon-based solid acid catalyst 1S-LC6-700.

[0030] (2) 200 mesh automobile waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 1300 KW / m 2 The light flux density was used to heat it to 700°C and maintain it for 2 hours. After the reaction, the pyrolysis oil obtained by condensation was collected, and the pyrolysis oil yield was 78.5wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 93.2wt.%, as shown in Table 1.

[0031] Embodiment 4:

[0032] (1) The organic waste leather of scrapped automobiles was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 800°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 12 hours. After the reaction was completed, it was naturally cooled and taken out and ground. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL of dichloromethane (CH2Cl2, AR, 99.5%) and 2mL of chlorosulfonic acid (ClHSO3, AR, 99%) were added to 1g of biochar, and the reaction was stirred at 65°C for 12 hours, and then washed, filtered, and dried to obtain a carbon-based solid acid catalyst 2S-LC12-800.

[0033] (2) 200 mesh automobile waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:5 and placed in a reactor at 1500 KW / m 2The light flux density was used to heat it to 900°C and maintain it for 3 hours. After the reaction, the pyrolysis oil obtained by condensation was collected, and the pyrolysis oil yield was 76.6wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 90.1wt.%, as shown in Table 1.

[0034] Embodiment 5:

[0035] (1) The scrapped car organic dismantling waste leather was placed in a quartz boat and sent into a tube furnace. The waste leather was carbonized at 400°C at a heating rate of 10°C / min for 1 hour under an inert atmosphere. After the reaction was completed, it was naturally cooled and then taken out and ground. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12h and then taken out and ground to obtain biochar. 20mL of dichloromethane (CH2Cl2, AR, 99.5%) and 0.5mL of chlorosulfonic acid (ClHSO3, AR, 99%) were added to 1g of biochar, and the reaction was stirred at 65°C for 12h, followed by washing, filtering and drying to obtain a carbon-based solid acid catalyst 0.5S-LC1-400.

[0036] (2) 200 mesh automobile waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:0.5 and placed in a reactor at 1000 KW / m 2 The light flux density was used to heat it to 400°C and maintain it for 2 hours. After the reaction, the pyrolysis oil obtained by condensation was collected, and the yield of pyrolysis oil was 8.6wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 10.2wt.%, as shown in Table 1.

[0037] Embodiment 6:

[0038] (1) The organic waste leather of scrapped automobiles was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 700°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 6 hours. After the reaction was completed, it was naturally cooled and taken out and ground. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL of dichloromethane (CH2Cl2, AR, 99.5%) and 1mL of chlorosulfonic acid (ClHSO3, AR, 99%) were added to 1g of biochar, and the reaction was stirred at 65°C for 12 hours, and then washed, filtered, and dried to obtain a carbon-based solid acid catalyst 1S-LC6-700.

[0039] (2) 200 mesh automobile waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 800 kW / m 2The light flux density was used to heat it to 700°C and maintain it for 0.5h. After the reaction, the pyrolysis oil obtained by condensation was collected and the yield of pyrolysis oil was 63.6wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 80.9wt.%, as shown in Table 1.

[0040] Embodiment 7:

[0041] (1) The organic waste leather of scrapped automobiles was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 700°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 6 hours. After the reaction was completed, it was naturally cooled and taken out and ground. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL of dichloromethane (CH2Cl2, AR, 99.5%) and 1mL of chlorosulfonic acid (ClHSO3, AR, 99%) were added to 1g of biochar, and the reaction was stirred at 65°C for 12 hours, and then washed, filtered, and dried to obtain a carbon-based solid acid catalyst 1S-LC6-700.

[0042] (2) 50 mesh waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 1300 KW / m 2 The light flux density was used to heat it to 700℃ and maintain it for 1 hour. After the reaction, the pyrolysis oil obtained by condensation was collected and the pyrolysis oil yield was 67.5wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 82.2wt.%, as shown in Table 1.

[0043] Embodiment 8:

[0044] (1) The organic waste leather of scrapped automobiles was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 700°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 6 hours. After the reaction was completed, it was naturally cooled and taken out and ground. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL of dichloromethane (CH2Cl2, AR, 99.5%) and 1mL of chlorosulfonic acid (ClHSO3, AR, 99%) were added to 1g of biochar, and the reaction was stirred at 65°C for 12 hours, and then washed, filtered, and dried to obtain a carbon-based solid acid catalyst 1S-LC6-700.

[0045] (2) 200 mesh automobile waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 1300 KW / m 2The light flux density was used to heat it to 700°C and maintain it for 3 hours. After the reaction, the pyrolysis oil obtained by condensation was collected, and the pyrolysis oil yield was 72.0wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 83.7wt.%, as shown in Table 1.

[0046] Embodiment 9:

[0047] (1) The organic waste leather of scrapped automobiles was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 700°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 6 hours. After the reaction was completed, it was naturally cooled and taken out and ground. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL of dichloromethane (CH2Cl2, AR, 99.5%) and 1mL of chlorosulfonic acid (ClHSO3, AR, 99%) were added to 1g of biochar, and the reaction was stirred at 65°C for 12 hours, and then washed, filtered, and dried to obtain a carbon-based solid acid catalyst 1S-LC6-700.

[0048] (2) 150 mesh waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 1300 KW / m 2 The light flux density was used to heat it to 800°C and maintain it for 0.5h. After the reaction was completed, the pyrolysis oil obtained by condensation was collected, and the pyrolysis oil yield was 73.6wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 85.0wt.%, as shown in Table 1.

[0049] Embodiment 10:

[0050] (1) The organic waste leather of scrapped automobiles was placed in a quartz boat and sent into a tube furnace. The temperature was raised to 700°C at a heating rate of 10°C / min under an inert atmosphere for carbonization for 6 hours. After the reaction was completed, it was naturally cooled and taken out and ground. Then, the inorganic components were removed with a 10wt.% hydrofluoric acid solution, washed and filtered until the filtrate was neutral, and the filter cake was vacuum dried at 80°C for 12 hours and then taken out and ground to obtain biochar. 20mL of dichloromethane (CH2Cl2, AR, 99.5%) and 1mL of chlorosulfonic acid (ClHSO3, AR, 99%) were added to 1g of biochar, and the reaction was stirred at 65°C for 12 hours, and then washed, filtered, and dried to obtain a carbon-based solid acid catalyst 1S-LC6-700.

[0051] (2) 200 mesh automobile waste tire particles and the catalyst prepared in (1) were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 1300 KW / m 2The light flux density was used to heat it to 700°C and maintain it for 2 hours. After the reaction was completed, the carbon-based solid acid catalyst was sieved and recovered, and the acidification step in (1) was used to regenerate it to obtain a regenerated carbon-based solid acid catalyst. 200 mesh automobile waste tire particles and the regenerated carbon-based solid acid catalyst were uniformly mixed in a mass ratio of 1:2 and placed in a reactor at 1300KW / m 2 The light flux density was used to heat it to 700°C and maintain it for 2 hours. After the reaction, the pyrolysis oil obtained by condensation was collected, and the pyrolysis oil yield was 74.3wt.% based on mass calculation. The pyrolysis oil was sent to GC-MS for qualitative and quantitative analysis, and the aromatic content in the pyrolysis oil was 92.1wt.%, as shown in Table 1. Compared with Example 1, it can be seen that the catalyst mentioned in the present invention can restore good catalytic activity through regeneration.

[0052] Table 1

[0053]

[0054] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing high-quality pyrolysis oil by catalytic pyrolysis of waste tires based on concentrated solar heat source, characterized in that: The method comprises the following steps: (1) The organic residues of scrapped automobiles, waste sponges or waste leather particles are placed in a quartz boat and sent into a tube furnace. The temperature is raised to 400-800°C at a heating rate of 10°C / min under an inert atmosphere and kept warm for 1-12 hours to carbonize the particles. After the reaction is completed, the particles are naturally cooled and then taken out and ground. The particles are then placed in 1-12 wt.% hydrofluoric acid and stirred at room temperature for 4-8 hours to remove inorganic components. The particles are washed and filtered until the filtrate is neutral, and then dried and ground to obtain biochar. (2) loading the biochar prepared in step (1) with phosphate groups, specifically, the steps are as follows: adding the biochar to deionized water, then adding phosphoric acid, mixing and ultrasonically dispersing for 12 hours, then washing with deionized water and filtering, repeating three times, drying the filter cake and grinding it to obtain a carbon-based solid acid loaded with phosphate groups; Alternatively, the biochar prepared in step (1) is loaded with sulfonic acid groups, specifically, the steps are as follows: adding the biochar to dichloromethane, then adding chlorosulfonic acid, stirring and reacting at room temperature to 70° C. for 12 h, then washing with deionized water and filtering, repeating three times, drying the filter cake and grinding it to obtain a carbon-based solid acid loaded with sulfonic acid groups; Step (2) The mass volume ratio of biochar to phosphoric acid or chlorosulfonic acid is 1 g: (0.1-2) mL; (3) placing the carbon-based solid acid loaded with phosphoric acid groups or the carbon-based solid acid catalyst loaded with sulfonic acid groups prepared in step (2) and the waste tire particles of scrapped organic demolition residues in a reactor, adjusting the power of the concentrated solar energy simulation light source, heating the reactants at different energy flux densities under an inert atmosphere, discharging the pyrolysis products through the purge gas, and collecting the liquid products after condensation; the mass ratio of the waste tire to the carbon-based solid acid catalyst is 1:0.5-5; the light energy flux density of the concentrated solar energy pyrolysis is 500-1500KW / m 2 The pyrolysis temperature is 400-900°C and the pyrolysis time is 0.5-3h.

2. The method according to claim 1, characterized in that The particle size of waste tire particles is 50 to 200 mesh.

3. The method according to claim 1, characterized in that The drying in steps (1) and (2) is carried out in a vacuum drying oven at 75-85°C.

4. The method according to claim 1, characterized in that: The concentration of hydrofluoric acid in step (1) is 9-10 wt.%.

5. The method according to claim 1, characterized in that Step (2) is: loading the biochar prepared in step (1) with sulfonic acid groups. The specific steps are as follows: adding the biochar to dichloromethane, then adding chlorosulfonic acid, stirring the reaction at 60-70° C. for 12 hours, then washing with deionized water and filtering, repeating three times, drying the filter cake and grinding it to obtain a carbon-based solid acid loaded with sulfonic acid groups.