Preparation method of in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy
The preparation method of in-situ autogenous two-dimensional carbide dispersion strengthened and toughened molybdenum alloy solves the problem of insufficient performance of molybdenum alloy at room temperature and high temperature, achieves high strength, high elongation and high temperature stability of molybdenum alloy, and expands its application in Possibility of high temperature applications.
Patent Information
- Application Number
- CN202310238874.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-03-14
AI Technical Summary
Existing molybdenum alloys have insufficient strength and elongation at room temperature and high temperature, and traditional strengthening processes are difficult to improve their room temperature and high-temperature properties at the same time, limiting their application in high-temperature scenarios.
An in-situ autogenous two-dimensional carbide dispersion toughened molybdenum alloy preparation method is used, by dry mixing MoO2 and two-dimensional MAX ceramic materials in a dual-power mixer to perform high-temperature reduction, cold isostatic pressing, pressureless sintering and thermoplastic processing. , forming uniformly distributed nano-TiC0.67 particles, enhancing the density and mechanical properties of molybdenum grains.
It significantly improves the room temperature and high temperature tensile strength and elongation of molybdenum alloy, improves its high temperature stability and density, and expands its application range in high temperature scenarios.
Smart Images

Figure CN116287833B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder metallurgy, and particularly relates to a method for preparing an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy. Background Art
[0002] Molybdenum metal is one of the most widely used refractory metal materials in industry. Due to its high melting point (2620±20℃), high density (10.2g / cm 3 ), high elastic modulus (280-390 GPa), low linear thermal expansion coefficient (5.8×10 -6 ~6.2×10 -6 / K), high wear resistance, good electrical and thermal conductivity, good acid and alkali resistance and liquid metal corrosion resistance, etc. As high-temperature resistant structural materials and functional materials, molybdenum and its alloys have broad application prospects in various industrial fields such as steel, metallurgy, machinery, chemical industry, nuclear energy, electronics, aerospace, etc. Although molybdenum metal and its alloys have many performance advantages, their room temperature and high temperature strength are still insufficient to meet the demand for high temperature resistant structural materials with the rapid development of science and technology. In particular, the low room temperature ductility of molybdenum metal leads to its poor machinability, which seriously limits its industrial application.
[0003] Oxides (La2O3, Ce2O3, Y2O3, ZrO2, Al2O3) and carbides (TiC, ZrC, HfC, TaC) are commonly used to strengthen molybdenum alloys. For example, adding oxide Al2O3 to the molybdenum matrix can significantly improve the hardness and wear resistance of the molybdenum alloy. Adding La2O3 to the molybdenum matrix can prepare a high-strength and tough molybdenum alloy with a yield strength of 813MPa, and can also obtain a higher fracture toughness (121.5MPa·m 2 ) and elongation (37.5%). Adding rare earth oxides can also increase the recrystallization temperature of molybdenum alloys, making molybdenum alloys have better high-temperature creep resistance. If carbide TiC particles are added to the TZM alloy, it is found that adding 5vol.% TiC particles can increase the Vickers hardness of the alloy by 50%, and the bending strength by 46%, but the ductility of the alloy will decrease. Adding oxides to improve the performance of molybdenum alloys requires that the size of the oxide particles is at the nanometer level, and the particles are dispersed and evenly distributed inside the molybdenum grains. The process is relatively complex and the equipment requirements are high, making it difficult to achieve large-scale application. Adding carbides to improve high-temperature mechanical properties requires that the carbides themselves have a high melting point, high hardness, and high chemical stability. In addition, their performance is closely related to composition control, deformation process, and heat treatment process, which requires high requirements and is difficult to control.
[0004] The design principles of new high-performance molybdenum materials include: 1) improving low-temperature brittleness and reducing alloy DBTT; 2) increasing recrystallization temperature, improving mechanical properties and structural stability at high temperatures; 3) improving radiation embrittlement resistance. Traditional non-in-situ synthesized composite materials are often accompanied by the following disadvantages: residual pores, large grain size, non-uniform distribution of reinforcement phase, poor wettability, and weak interface between reinforcement phase and matrix.
[0005] M n+1 AX n The MAX phase (where M is an early transition metal, A is an A-group element, and X is C or N) is a layered hexagonal solid. The unique crystal structure of the MAX phase gives it unique chemical bond characteristics: M and X are bonded by strong covalent bonds and ionic bonds; M and A are bonded by weaker covalent bonds or metallic bonds, which makes it easy for the MAX phase to slip along the basal plane
[0001] . This unique bonding configuration enables it to combine many advantages of ceramic materials and metal materials, such as high modulus, low specific gravity, good electrical and thermal conductivity, machinability, thermal shock resistance, high damage tolerance, thermal stability, creep resistance and oxidation resistance. The existing strengthening process of molybdenum alloys, whether adding oxides or carbides, cannot simultaneously have high strength, high toughness and high-temperature stability at room temperature and high temperature, which restricts its application in high-temperature scenarios such as nuclear reactors. Therefore, in order to meet the requirements of use, it is necessary to further improve the comprehensive mechanical properties and high-temperature stability of molybdenum alloys. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy, so as to improve the room temperature and high temperature strength of the molybdenum alloy, increase its elongation, refine the powder particle size, further improve its density, and simultaneously improve the toughness and strength of the molybdenum alloy.
[0007] The present invention is specifically implemented by the following technical scheme. According to the preparation method of an in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy proposed by the present invention, the method comprises the following steps:
[0008] (1): According to the requirements of the final product, a certain amount of MoO2 and two-dimensional MAX ceramic material are weighed, dry mixed for 10 to 30 hours using a dual-power mixer, and sieved for later use;
[0009] (2): The powder prepared in step (1) is subjected to high-temperature reduction in a reducing gas hydrogen atmosphere, wherein the reduction temperature is 700 to 1000° C. and the hydrogen flow rate is 10 to 20 m 3 / h, reduction time 8-25h, powder spreading height ≤2 / 3, to prepare molybdenum alloy precursor powder;
[0010] (3): According to the required size of the final product, a suitable rubber mold is selected, a certain amount of the prepared molybdenum alloy precursor powder is weighed and loaded into the rubber mold, and a cold isostatic press is used for pressing;
[0011] (4): The green compact obtained in step (3) is subjected to pressureless sintering under a reducing gas, and after cooling in a furnace, a molybdenum alloy sintered green compact is obtained;
[0012] (5): heating the molybdenum alloy sintered blank prepared in step (4) to 1100-1600° C. in a protective hydrogen atmosphere (to prevent oxidation of molybdenum), keeping the temperature for 30-60 min, and then performing hot plastic processing;
[0013] (6): The molybdenum alloy billet prepared in step (5) is annealed in a protective hydrogen atmosphere (the purpose is to prevent molybdenum oxidation) to finally obtain a high-strength and tough molybdenum alloy, that is, an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy.
[0014] Preferably, the molybdenum dioxide used in step (1) has a particle size of 8 to 20 μm and a potassium impurity content of 5 to 10 ppm; the two-dimensional MAX ceramic material is a lamellar Ti3AlC2 with 3 to 10 layers, a purity of not less than 98%, and a particle size of 2 to 8 μm.
[0015] Furthermore, the particle size of the molybdenum alloy precursor powder obtained in step (2) is 1 to 2 μm.
[0016] Preferably, the pressure of the cold isostatic pressing of the compact in step (3) is 150-230 MPa, and the holding time is 10-30 min.
[0017] Preferably, the pressureless sintering temperature in step (4) is 1700-2100°C, the holding time is 6-10h, and the hydrogen flow rate is 8-15m 3 / h, and after cooling in the furnace, a molybdenum alloy sintered billet is obtained.
[0018] Furthermore, in step (5), the thermoplastic processing is one or a combination of rotary forging, rolling, extrusion or drawing; the total number of passes of the thermoplastic processing is 3 to 10 times, the deformation amount of each pass is 15 to 25%, and the total deformation amount is ≥50%.
[0019] Preferably, the annealing temperature of step (6) is 900-1500° C., and the holding time is 30-200 min.
[0020] Furthermore, the prepared in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy includes molybdenum grains and nano-TiC uniformly distributed in the molybdenum grains. 0.67 Among them, the average particle size of the molybdenum grains is 10 to 20 μm, and the nano-TiC is evenly distributed inside the molybdenum grains. 0.67 The average particle size is 0.5 to 3 μm.
[0021] The present invention can also replace MoO2 with WO3 according to the above method to prepare an in-situ self-generated two-dimensional carbide dispersion-strengthened tungsten alloy; or replace MoO2 with CuO to prepare an in-situ self-generated two-dimensional carbide dispersion-strengthened copper alloy; or replace MoO2 with NiO to prepare an in-situ self-generated two-dimensional carbide dispersion-strengthened nickel alloy, thereby expanding the application of the present invention.
[0022] Furthermore, the two-dimensional MAX ceramic material in step (1) can also be any one or more of Zr3AlC2, Si3AlC2, Hf3AlC2, Zr2AlC, Si2AlC, Hf2AlC2, Zr4AlC3, Si4AlC3, and Hf4AlC3, and is not limited to Ti3AlC2.
[0023] Compared with the prior art, the present invention has obvious advantages and beneficial effects, and has at least the following advantages:
[0024] (1) The present invention uses a MAX phase material with a high melting point, high hardness, and high fracture toughness as a doping phase. By controlling the mass ratio of molybdenum dioxide and two-dimensional MAX material, the initial powder is subjected to hydrogen reduction, cold isostatic pressing, hydrogen pressureless sintering, thermoplastic treatment, and annealing to obtain a high-strength and tough molybdenum alloy. The reinforcing phase MAX material selectively etches away Al under high-temperature sintering, and the original ternary layered structure is decomposed into Al and two-dimensional MXene material (TiC 0.67 ), Al generates alumina by absorbing impurity oxygen, and the alumina particles and carbides generated by in-situ reaction decomposition are dispersed in the molybdenum matrix. Among them, the in-situ decomposed Al generates alumina by absorbing impurity oxygen to reduce the brittleness of the alloy, while the other in-situ generated Mxene particles are finer, have a large specific surface area and high surface energy, can promote the densification of the material, thereby improving the yield strength and fracture toughness of the molybdenum alloy and other mechanical properties; and the Mxene particles generated by the in-situ reaction have better thermal stability, are mainly distributed on the grain boundaries, and effectively hinder the movement and deformation of the grain boundaries at high temperatures, thereby making the material microstructure more stable at high temperatures, so that the molybdenum alloy has good high temperature strength and high recrystallization temperature, thereby improving the performance of the molybdenum alloy in high temperature scenarios and expanding the application range of the molybdenum alloy.
[0025] (2) The morphology and particle size of molybdenum powder have hereditary effects on the performance of molybdenum alloy. According to the concept of heredity in biology, the morphological evolution of particle agglomerates has obvious hereditary phenomena and is accompanied by a certain degree of variation. For the morphology of single particles, each generation has its own intrinsic characteristics, and variation is dominant, and there is basically no hereditary phenomenon. The hereditary characteristics of Fisher's particle size are that the raw material particles are coarser, and the corresponding product particles are also coarser; the raw material particles are finer, and the corresponding product particles are also finer. The inheritance of impurity elements also has obvious characteristics. Volatile and easily contaminated elements are mainly subject to variation during the reduction process, while other impurity elements that are not volatile and do not pollute are mainly subject to inheritance. The present invention introduces fine secondary phase elements into MoO2 to break the hereditary nature of particle agglomerates. In the process of controlling the reduction of MoO2 to Mo, internal diffusion is dominant, and the apparent activation energy of this step is 30.1 kJ / mol. The transformation of small particle MoO2 follows the chemical vapor migration model. Due to the introduction of secondary phases, Mo powder is overburned, the edges are arced, and the molybdenum powder is nearly spherical. The present invention prepares fine and uniform molybdenum powder, the powder has a Fisher particle size of 1-2 μm and a loose density of 0.7-0.9 g / cm 3 .
[0026] (3) The present invention can further refine the grains and improve the density and performance of the molybdenum alloy through the thermoplastic deformation process. The microstructure of the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy prepared by the above method includes molybdenum grains and nano-TiC uniformly distributed in the molybdenum grains. 0.67 Among them, the average width of the molybdenum grains is 10 to 20 μm, and the nano-TiC is evenly distributed inside the molybdenum grains. 0.67 The average particle size of the particles is 0.5 to 3 μm.
[0027] (4) The molybdenum alloy of the present invention has excellent comprehensive properties, outstanding high-temperature performance, and a green and efficient preparation method. It can be mass-produced and can produce large-size products. It has great industrial application value and will have very good application prospects in nuclear reactors, key aerospace components, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is a SEM image of the molybdenum alloy precursor powder prepared in Example 1;
[0029] Figure 2 is an optical microscopic metallographic image of the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy prepared in Example 1;
[0030] Figure 3 is an optical microscopic metallographic image of the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy prepared in Example 2;
[0031] Figure 4is an optical microscopic metallographic image of the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy prepared in Example 3;
[0032] Figure 5 The stress-strain curves of the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy and pure molybdenum prepared in Examples 1 to 3;
[0033] Figure 6 It is the high temperature stress-strain curve of the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy and pure molybdenum prepared in Examples 1 to 3 at 1200°C. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The preparation method of the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy provided by the present invention mainly comprises the following steps:
[0036] (1): According to the requirements of the final product, a certain amount of MoO2 and Ti3AlC2 powders are weighed, dry-mixed for 10 to 30 hours using a dual-power mixer, and sieved for later use; the molybdenum dioxide used has a particle size of 8 to 20 μm, and the content of impurity potassium is 5 to 10 ppm; Ti3AlC2 is lamellar, with 3 to 10 layers, a purity of not less than 98%, and a particle size of 2 to 8 μm;
[0037] (2) The powder prepared in step (1) is subjected to high-temperature reduction in a reducing gas hydrogen atmosphere, wherein the reduction temperature is 700 to 1000° C. and the hydrogen flow rate is 10 to 20 m / s. 3 / h, reduction time 8-25h, powder spreading height ≤2 / 3, to prepare molybdenum alloy precursor powder with a particle size of 1-2μm;
[0038] (3): According to the required size of the final product, a suitable rubber mold is selected, a certain amount of the prepared molybdenum alloy precursor powder is weighed and loaded into the rubber mold, and a cold isostatic press is used for pressing, with a pressure of 150 to 230 MPa and a holding time of 10 to 30 minutes.
[0039] (4): The compact obtained in step (3) is subjected to pressureless sintering in the presence of reducing gas hydrogen at a sintering temperature of 1700 to 2100° C., a holding time of 6 to 10 h, and a hydrogen flow rate of 8 to 15 m 3 / h, and after cooling in the furnace, a molybdenum alloy sintered blank is obtained; the particle size of the molybdenum crystal grains in the molybdenum alloy is about 20 to 50 μm;
[0040] (5): The molybdenum alloy blank prepared in step (4) is heated to 1100-1500° C. in a protective gas hydrogen atmosphere (to prevent molybdenum oxidation), kept warm for 15-60 min, and then subjected to thermoplastic processing, wherein the thermoplastic processing is one or a combination of rotary forging, rolling, extrusion or drawing, wherein the total number of passes of the thermoplastic deformation processing is 3-10 times, the deformation amount of each pass is 15-25%, and the total deformation amount is ≥50%.
[0041] (6): The molybdenum alloy billet prepared in step (5) is annealed in a protective gas hydrogen atmosphere at a temperature of 900 to 1500° C. for 30 to 200 min, thereby finally obtaining a high-strength and tough molybdenum alloy, i.e., an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy.
[0042] The microstructure of the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy prepared by the above method includes molybdenum grains and nano-TiC uniformly distributed in the molybdenum grains. 0.67 Among them, the average width of the molybdenum grains is 10 to 20 μm, and the nano-TiC is evenly distributed inside the molybdenum grains. 0.67 The average particle size of the particles is 0.5 to 3 μm.
[0043] As further preferred, in step (1), the mass of MoO2 accounts for 95-99.5% of the total mass of the mixed powder of MoO2 and Ti3AlC2, and the mass of Ti3AlC2 accounts for 0.5-5% of the total mass of the mixed powder of MoO2 and Ti3AlC2.
[0044] The present invention adopts the above method to obtain an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy. In other embodiments, the two-dimensional MAX ceramic material Ti3AlC2 can be replaced by any one or more of 312 phase MAX phase ceramics (Zr3AlC2 or Si3AlC2 or Hf3AlC2), 211 phase MAX phase ceramics (Zr2AlC or Si2AlC or Hf2AlC2) and 413 phase MAX phase ceramics (Zr4AlC3 or Si4AlC3 or Hf4AlC3), and an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy can also be obtained, except that the reinforcing phase carbide is changed. For those skilled in the art, the replacement scheme is easy to understand and will not be repeated in the present invention.
[0045] At the same time, by replacing the raw material MoO2, the above method can also be used to prepare in-situ self-generated two-dimensional carbide dispersion-strengthened tungsten alloy, copper alloy or nickel alloy. For example, the metal matrix material for preparing the in-situ self-generated two-dimensional carbide dispersion-strengthened tungsten alloy can be WO3, the metal matrix material for preparing the in-situ self-generated two-dimensional carbide dispersion-strengthened copper alloy can be CuO, and the metal matrix material for preparing the in-situ self-generated two-dimensional carbide dispersion-strengthened nickel alloy can be NiO. The preparation method is the same as the preparation method of the above-mentioned in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy, and the present invention will not repeat it again.
[0046] The following is a detailed description with specific embodiments:
[0047] Example 1
[0048] (1): According to the requirements of the final product, 99 parts of MoO2 and 1 part of Ti3AlC2 powder were put into a dual-power mixer and dry mixed for 20 hours, and then passed through a 300-mesh sieve for later use;
[0049] (2): The powder obtained in step (1) is subjected to high-temperature reduction in a reducing gas hydrogen atmosphere, with a reduction temperature of 800°C and a hydrogen flow rate of 18 m 3 / h, reduction time 22h, powder spreading height 2 / 3, to prepare molybdenum alloy precursor powder with a particle size of 1-2μm;
[0050] (3): According to the required size of the final product, a suitable rubber mold is selected, a certain amount of the prepared molybdenum alloy precursor powder is weighed and loaded into the rubber mold, and a cold isostatic press is used for pressing, with a pressure of 200 MPa and a holding time of 15 min.
[0051] (4): The pressed green sheet obtained in step (3) is subjected to pressureless sintering in the presence of reducing gas hydrogen at a sintering temperature of 2000° C. for a holding time of 10 h, and then cooled in the furnace to obtain a molybdenum alloy sintered green sheet; the particle size of the molybdenum grains in the molybdenum alloy is about 35 to 50 μm;
[0052] (5): The molybdenum alloy billet prepared in step (4) is heated to 1200° C. in a protective hydrogen atmosphere, kept warm for 60 minutes, and then subjected to thermoplastic processing, wherein the thermoplastic processing is rolling. The total number of passes of the thermoplastic deformation processing is 5 times, the deformation amount of each pass is 25%, and the total deformation amount is 76.23%.
[0053] (6): The molybdenum alloy blank prepared in step (5) is annealed in a protective hydrogen atmosphere at a temperature of 1000° C. for 160 min, and finally a high-strength and tough molybdenum alloy is obtained, namely, an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy having a particle size of 12 to 20 μm and a secondary phase TiC uniformly dispersed in the molybdenum grains. 0.67The particle size of the particles is 0.5 to 3 μm, and the density of the molybdenum alloy is 99%.
[0054] The room temperature mechanical properties of the in-situ two-dimensional carbide dispersion-strengthened molybdenum alloy prepared in this embodiment were tested using an American INSTRON-5967 universal testing machine, and its high temperature compressive strength was tested using an American Gleeble-1500D thermal simulation testing machine. The room temperature tensile strength of the in-situ two-dimensional carbide dispersion-strengthened molybdenum alloy obtained in this embodiment was 809 MPa, the elongation was 47.8%, and the high temperature compressive strength at 1200°C was 320 MPa, which were improved by 72.1%, 91.2% and 113.3% respectively compared with pure molybdenum metal, thereby increasing the plastic toughness of the molybdenum alloy without reducing its strength.
[0055] Figure 1 This is a morphology picture of the molybdenum alloy precursor powder prepared in step (2) of this embodiment. It can be seen that the powder is a nearly spherical powder with a diameter of 1 to 2 μm.
[0056] Figure 2 This is the organizational morphology (optical microscopy metallographic image) of the in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy prepared in this embodiment. The molybdenum alloy particle size is 12 to 20 μm, the larger secondary phase is evenly distributed at the grain boundaries, and the fine secondary phase particles are evenly distributed inside the grains.
[0057] Example 2
[0058] (1): According to the requirements of the final product, 98.5 parts of MoO2 and 1.5 parts of Ti3AlC2 powder were put into a dual-power mixer and dry mixed for 20 hours, and then passed through a 300-mesh sieve for later use;
[0059] (2): The powder obtained in step (1) is subjected to high-temperature reduction in a reducing gas hydrogen atmosphere, the reduction temperature is 900°C, the hydrogen flow rate is 20m 3 / h, reduction time 18h, powder spreading height ≤ 2 / 3, to prepare molybdenum alloy precursor powder with a particle size of 1 to 2 μm;
[0060] (3): According to the required size of the final product, a suitable rubber mold is selected, a certain amount of the prepared molybdenum alloy precursor powder is weighed and loaded into the rubber mold, and a cold isostatic press is used for pressing, with a pressure of 200 MPa and a holding time of 15 min.
[0061] (4): The pressed green sheet obtained in step (3) is subjected to pressureless sintering in the presence of reducing gas hydrogen at a sintering temperature of 1900° C. for a holding time of 10 h, and then cooled in the furnace to obtain a molybdenum alloy sintered green sheet; the particle size of the molybdenum grains in the molybdenum alloy is about 25 to 35 μm;
[0062] (5): The molybdenum alloy billet prepared in step (4) is heated to 1300° C. in a protective hydrogen atmosphere (to prevent oxidation of molybdenum), kept warm for 60 minutes, and then subjected to thermoplastic processing. The thermoplastic processing is one or a combination of rotary forging, rolling, extrusion or drawing. The total number of passes of the thermoplastic deformation processing is 8 times, the deformation amount of each pass is 20%, and the total deformation amount is 83.22%.
[0063] (6): The molybdenum alloy blank prepared in step (5) is annealed in a protective hydrogen atmosphere at a temperature of 1100° C. for 160 min, and finally a high-strength and tough molybdenum alloy is obtained, namely, an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy having a particle size of 10 to 15 μm and a secondary phase TiC uniformly dispersed in the molybdenum grains. 0.67 The particle size of the particles is 0.5 to 3 μm, and the density of the molybdenum alloy is 99.2%.
[0064] The room temperature mechanical properties and high temperature compressive strength of the in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy prepared in this embodiment were tested by the method described in Example 1. The room temperature tensile strength was 1024 MPa, the elongation was 48.5%, and the high temperature compressive strength at 1200°C was 335 MPa, which were respectively increased by 118%, 94% and 123.3% compared with pure molybdenum metal, thereby increasing the plastic toughness of the molybdenum alloy without reducing the strength.
[0065] Figure 3 This is the organizational morphology (optical microscopy metallographic image) of the in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy prepared in this embodiment. The molybdenum alloy particle size is 10-15 μm, the larger secondary phase is evenly distributed at the grain boundaries, and the fine secondary phase particles are evenly distributed inside the grains.
[0066] Example 3
[0067] (1): According to the requirements of the final product, 98 parts of MoO2 and 2 parts of Ti3AlC2 powder were put into a dual-power mixer and dry mixed for 20 hours, and then passed through a 300-mesh sieve for later use;
[0068] (2): The powder obtained in step (1) is subjected to high-temperature reduction in a reducing gas hydrogen atmosphere, with a reduction temperature of 1000°C and a hydrogen flow rate of 15 m / s. 3 / h, reduction time 20h, powder spreading height ≤ 2 / 3, to prepare molybdenum alloy precursor powder with a particle size of 1 to 2μm;
[0069] (3): According to the required size of the final product, a suitable rubber mold is selected, a certain amount of the prepared molybdenum alloy precursor powder is weighed and loaded into the rubber mold, and a cold isostatic press is used for pressing, with a pressure of 200 MPa and a holding time of 15 min.
[0070] (4): The pressed green sheet obtained in step (3) is subjected to pressureless sintering in the presence of reducing gas hydrogen at a sintering temperature of 1800° C. for a holding time of 10 h, and then cooled in the furnace to obtain a molybdenum alloy sintered green sheet; the particle size of the molybdenum grains in the molybdenum alloy is about 20 to 35 μm;
[0071] (5): The molybdenum alloy billet prepared in step (4) is heated to 1400° C. in a protective hydrogen atmosphere (to prevent oxidation of molybdenum), kept warm for 60 minutes, and then subjected to thermoplastic processing, wherein the thermoplastic processing is one or a combination of rotary forging, rolling, extrusion or drawing, wherein the total number of passes of the thermoplastic deformation processing is 10 times, the deformation amount of each pass is 25%, and the total deformation amount is 94.5%.
[0072] (6): The molybdenum alloy blank prepared in step (5) is annealed in a protective hydrogen atmosphere at a temperature of 1300° C. for 160 min, and finally a high-strength and tough molybdenum alloy is obtained, namely, an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy having a particle size of 10 to 12 μm and a secondary phase TiC uniformly dispersed in the molybdenum grains. 0.67 The particle size of the particles is 0.5 to 3 μm, and the density of the molybdenum alloy is 99.4%.
[0073] The room temperature mechanical properties and high temperature compressive strength of the in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy prepared in this embodiment were tested by the method described in Example 1. The room temperature tensile strength was 1305 MPa, the elongation was 47.9%, and the high temperature compressive strength at 1200°C was 415 MPa, which were respectively increased by 177.6%, 91.6% and 176.6% compared with pure molybdenum metal, thereby increasing the plastic toughness of the molybdenum alloy without reducing the strength.
[0074] Figure 4 This is the organizational morphology (optical microscopy metallographic image) of the in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy prepared in this embodiment. The molybdenum alloy particle size is 10-12 μm, the larger secondary phase is evenly distributed at the grain boundaries, and the fine secondary phase particles are evenly distributed inside the grains.
[0075] Comparative Example 1
[0076] In step (1), Ti3AlC2 is not added, and the other steps are the same as in Example 1 to obtain a molybdenum product. The product is tested according to the testing method of Example 1. The prepared pure molybdenum has a particle size of 70 to 100 μm, a density of 96%, a room temperature tensile strength of 470 MPa, an elongation of 25%, and a high temperature compressive strength of 150 MPa at 1200°C.
[0077] Figure 5 3 and 4. The stress-strain curves of the in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy obtained in each embodiment and the pure molybdenum obtained in Comparative Example 1 are shown in FIG. 3 . The tensile strength of the molybdenum alloys obtained by different processes in the embodiments is slightly different, but is generally higher than that of pure molybdenum.
[0078] Figure 6 The stress-strain curves of the in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloys obtained in each embodiment and the pure molybdenum obtained in Comparative Example 1 at 1200°C are shown. The compressive strength of the molybdenum alloys obtained by different processes in the embodiments at 1200°C is greatly improved compared with that of pure molybdenum.
[0079] Comparative Example 2
[0080] Molybdenum dioxide and lanthanum oxide are added in step (1), and the other steps are the same as in Example 1 to obtain a molybdenum product. The prepared molybdenum alloy has a particle size of 30 to 50 μm, a density of 97%, a room temperature tensile strength of 653 MPa, an elongation of 20%, and a high temperature compressive strength of 210 MPa at 1200°C. Compared with the pure molybdenum in Comparative Example 1, the strength is improved, but the plasticity and toughness are poor.
[0081] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy, characterized in that The following steps are involved: (1): According to the requirements of the final product, a certain amount of MoO2 and Ti3AlC2 are weighed, dry-mixed for 10 to 30 hours using a dual-power mixer, and sieved for use. The particle size of the MoO2 is 8 to 20 µm; the Ti3AlC2 is lamellar, with 3 to 10 layers and a particle size of 2 to 8 µm; the mass of MoO2 accounts for 95 to 99.5% of the total mass of the mixed powder of MoO2 and Ti3AlC2, and the mass of Ti3AlC2 accounts for 0.5 to 5% of the total mass of the mixed powder of MoO2 and Ti3AlC2; (2): The powder prepared in step (1) is subjected to high-temperature reduction in a hydrogen atmosphere at a reduction temperature of 700-1000°C and a hydrogen flow rate of 10-20 m 3 / h, reduction time 8-25h, powder spreading height ≤2 / 3, to prepare molybdenum alloy precursor powder; (3): According to the required size of the final product, select a suitable rubber mold, weigh a certain amount of the prepared molybdenum alloy precursor powder and put it into the rubber mold, and use a cold isostatic press to press the blank; (4): The compact obtained in step (3) is subjected to pressureless sintering at 1700-2100°C in a hydrogen atmosphere for 6-10 hours at a hydrogen flow rate of 8-15 m 3 / h, and after cooling in the furnace, a molybdenum alloy sintered blank is obtained; (5): heating the molybdenum alloy sintered blank obtained in step (4) to 1100-1600° C. in a hydrogen atmosphere, keeping the temperature for 30-60 min, and then performing thermoplastic processing; the thermoplastic processing is one or a combination of rotary forging, rolling, extrusion or drawing; the total number of thermoplastic processing passes is 3-10 times, the deformation amount of each pass is 15-25%, and the total deformation amount is ≥50%; (6): The molybdenum alloy blank obtained in step (5) is annealed at 900-1500°C in a hydrogen atmosphere for 30-200 min to finally obtain an in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy, which includes molybdenum grains and nano-TiC uniformly distributed in the molybdenum grains. 0.67 The average particle size of molybdenum grains is 10-20 μm, and the nano-TiC 0.67 The average particle size is 0.5~3μm; the in-situ self-generated two-dimensional carbide dispersion-strengthened molybdenum alloy has a high temperature compressive strength of 320~415 MPa at 1200℃, a density of 99%, a room temperature tensile strength of 809MPa, and an elongation of 47.8%, or a density of 99.2%, a room temperature tensile strength of 1024MPa, and an elongation of 48.5%, or a density of 99.4%, a room temperature tensile strength of 1305MPa, and an elongation of 47.9%.
2. The method for preparing the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy according to claim 1, characterized in that The particle size of the molybdenum alloy precursor powder obtained in step (2) is 1 to 2 μm.
3. The method for preparing the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy according to claim 1, characterized in that In step (3), the pressure of the cold isostatic pressing of the compact is 150 to 230 MPa, and the holding time is 10 to 30 minutes.
4. The method for preparing the in-situ self-generated two-dimensional carbide dispersion toughened molybdenum alloy according to claim 1, characterized in that According to the above method, MoO2 is replaced with WO3 to prepare an in-situ self-generated two-dimensional carbide dispersion-strengthened tungsten alloy; Or replace MoO2 with CuO to prepare in-situ self-generated two-dimensional carbide dispersion-strengthened copper alloy; Or replace MoO2 with NiO to prepare in-situ self-generated two-dimensional carbide dispersion-strengthened nickel alloy.
Citation Information
Patent Citations
Roller for continuous induction type rapid quenching furnace and manufacturing method of roller
CN112792308A
MAX phase reinforced tungsten / molybdenum fine grain alloy and preparation method thereof
CN113667854A
Preparation method of double-peak grain molybdenum alloy
CN114277274A