A heat-resistant 7-series aluminum alloy containing Mo element and free of coarse grains and preparation method thereof

By using semi-continuous casting and multi-stage heat treatment technology in 7-Series aluminum alloys, molybdenum, zirconium and scandium elements are solidly dissolved inside the grains and form high-temperature reinforced phases, the problem of poor heat resistance of 7-Series aluminum alloys is solved and improved The heat resistance and mechanical properties of aluminum alloys reduce the occurrence of rough crystallization on the surface of the wheel.

CN118600291BActive Publication Date: 2024-11-19D MAG KUNSHAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073654.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Due to poor heat resistance during thermal deformation, 7-Series aluminum alloys have coarse recrystallization when high-temperature energy storage is released, reducing product life and mechanical properties. At the same time, the existing technology lacks Mo-containing aluminum alloys that meet the wheel properties.

Method used

The ingots were prepared by semi-continuous casting, with a cooling rate of 10K/S~105K/S, so that molybdenum (Mo), zirconium (Zr), scandium (Sc) elements were forced to dissolve inside the grains, forming AlMo3, Al12Mo, and Al3 ( Sc, Zr) metal compounds improve the high-temperature reinforced phase distribution of the alloy through three-stage homogenization, reduce the tendency of coarse recrystallization, and improve the mechanical properties through multi-stage heat treatment and surface treatment.

Benefits of technology

It effectively improves the room temperature strength and heat resistance of 7-Series aluminum alloy, extends the recrystallization temperature, reduces the appearance of coarse crystal structure on the wheel surface, and improves the service life and mechanical properties of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118600291B_ABST
    Figure CN118600291B_ABST
Patent Text Reader

Abstract

The present invention discloses a heat-resistant 7 series aluminum alloy containing Mo element and free of coarse grains, and a preparation method thereof. The mass percentages of the materials are as follows: Zn: 5.10-6.50%; Mg: 1.10-2.30%; Cu: 1.10-2.30%; Zr: 0.10-0.25%; Mo: 0.05-0.20%; Sc: 0.05-0.15%; Ti: 0.02-0.04; Fe≤0.15; Si≤0.10, and the ratio of Zr / Sc is 2:1-3:1, and the balance is Al. The present invention adds elements of molybdenum, zirconium and scandium, and in the homogenization process, the molybdenum, zirconium and scandium elements form dispersed high-temperature strengthening phase particles with a size range of 5-20µm in the grains. The strengthening phase particles have high-temperature stability, play a role in pinning the dislocation of the 7 series alloy at high temperatures, improve the heat resistance, and improve the stability and reliability of the product in a high-temperature environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal materials and material processing, and in particular to a heat-resistant 7-series aluminum alloy containing Mo element and free of coarse grains, and a preparation method thereof. Background Art

[0002] Aluminum alloy materials are the most widely used metal materials at present due to their advantages such as light weight, high strength and good plasticity. Therefore, producing a 7 series aluminum alloy with high heat resistance is of great significance for lightweighting. The 7 series aluminum alloy is a series of heat-treatable and strengthened aluminum alloys with high strength, good toughness and good machinability. However, during the thermal deformation process, the 7 series alloy has poor heat resistance and large internal metal resistance, so the high-temperature energy storage is high. In the subsequent thermal processing and heat treatment stages, the release of high-temperature energy storage causes coarse recrystallization on the profile surface. This phenomenon of coarse recrystallization will not only reduce the service life and mechanical properties of the product, but also cause color difference on the surface after anodizing, seriously affecting the surface quality of the product.

[0003] Adding elements such as Sc and Zr can improve the heat resistance of aluminum alloys. In aluminum alloys, the strength and toughness of the alloys can be improved through fine grain strengthening, limited solid solution strengthening and second phase strengthening. It can also improve the corrosion resistance and processing properties of aluminum alloys, but it will increase its cost.

[0004] Adding an appropriate amount of Mo element to aluminum alloy can not only improve the strength and heat resistance of the alloy, strengthen fine grains, thereby reducing the tendency of coarse recrystallization of the product, but also reduce costs. Patent CN108998710A discloses a process for preparing aluminum alloy for mobile phone shells, using rare earth elements with a Mo content of 1% to 2% to improve the vibration reduction and noise reduction performance of Al alloys, and improve the strength and plasticity of the alloy. However, there is no Mo-containing aluminum alloy that meets the properties of wheels in the prior art. Summary of the invention

[0005] In view of the above technical problems, the purpose of the present invention is to provide a heat-resistant 7-series aluminum alloy containing Mo element without coarse grains and a preparation method thereof. The ingot is prepared by semi-continuous casting, and the cooling rate of the ingot is 10K / S to 105K / S, so that the molybdenum (Mo), zirconium (Zr), and scandium (Sc) elements are forced to dissolve in the grains, and then a three-stage homogenization is used to make the high-temperature element Mo (Mo) form AlMo3, Al2O3, and Al3O3 in the 7-series aluminum alloy. 12The dispersed high temperature strengthening phase of Mo and Al3 (Sc, Zr) metal compounds has a size of 5 to 20µm when the alloy solidifies normally, which effectively improves the room temperature strength and heat resistance of the alloy, thereby improving the heat resistance of the 7 series aluminum alloy. In addition, adding trace amounts of transition metal zirconium (Zr) and scandium (Sc) to the 7 series alloy can refine the grain structure of the cast rod, promote the formation of the aging transition phase, improve the stability of the GP zone and the transition phase, improve the aging hardening characteristics of the alloy, greatly improve the mechanical properties of the alloy, and increase the recrystallization temperature of hot deformation, so that the product does not have a surface coarse grain structure.

[0006] To achieve the above object, the specific technical solutions of the present invention are as follows:

[0007] The present invention provides a 7 series aluminum alloy containing Mo element, which is free of coarse grains and heat-resistant. The aluminum alloy material contains the following element components by mass percentage: Zn: 5.10-6.50%; Mg: 1.10-2.30%; Cu: 1.10-2.30%; Zr: 0.10-0.25%; Mo: 0.05-0.20%; Sc: 0.05-0.15%; Ti: 0.02-0.04; Fe≤0.15; Si≤0.10; and the ratio of Zr / Sc is 2:1-3:1, the balance is Al, and the unspecified elements are regarded as impurity elements with a content of less than 0.01%. The alloy is used to prepare a wheel hub, and the tensile strength is 600MPa-650MPa, the yield strength is 550MPa-600MPa, and the elongation is 10%-14%.

[0008] The present invention also provides a method for preparing a heat-resistant 7-series aluminum alloy containing Mo element and free of coarse grains, which comprises smelting and casting treatment, gradient homogenization treatment, reverse extrusion, rounding, welding, multi-stage heat treatment and surface treatment.

[0009] Preferably, the smelting and casting process adopts the following method: select Zn, Mg, Cu, Zr, Mo, Sc and pure aluminum ingots according to the mass percentage requirements for batching and melting. First, the melt temperature is maintained in the range of 730-770°C, the aluminum melt needs to be refined, slag-stripped, and the melt is degassed and filtered using rotor online degassing and plate filtration to make the melt hydrogen content less than 0.12mL / 100gAl, hydraulic semi-continuous casting rods are used, the ingot cooling rate is 10K / S-105K / S, the ingot internal inclusions are less than 0.1mm, and the cast rod diameter control range is 90mm-178mm.

[0010] Preferably, the gradient homogenization treatment adopts the following method: a three-stage homogenization process is adopted, in which the temperature is raised from room temperature to 200-300°C for 5-10 hours to form AlMo3, Al 12Mo and Al3 (Sc, Zr) disperse and precipitate high-temperature strengthening phases with good thermal stability. The dispersed distribution of these high-temperature strengthening phases can hinder grain boundary sliding and dislocation movement, and improve the stability of the matrix structure. In the second stage, the temperature is continuously raised to 400-450℃ and kept for 1-5 hours to promote the dissolution of Zn, Mg, and Cu strengthening phase particles to improve strength. In the third stage, the temperature is continuously raised to 450-500℃ and kept for 15-30 hours to optimize Al3 (Sc, Zr) and AlMo3, Al 12 The distribution of Mo in the alloy makes AlMo3, Al 12 The heat-resistant Mo phase and Al3 (Sc, Zr) phase are further dissolved into the aluminum matrix, thereby reducing segregation, improving the heat resistance of the alloy, and more effectively increasing the recrystallization temperature. After the heat treatment is completed, it is cooled to room temperature at a rate of 200℃ / h~300℃ / h to prevent the precipitation and coarsening of the solid solution phase particles after homogenization, which affects the subsequent process technology.

[0011] Preferably, the reverse extrusion adopts the following method: the ingot after homogenization treatment is heated to 320℃~350℃, reverse extrusion is adopted, the extrusion ratio is 30~70, and the aluminum ingot is heated in a direct fire furnace. Specifically, the heating temperature is 320℃~350℃, the heating time is 2~5h before loading, the ingot barrel temperature is 350℃~450℃, the extrusion speed is 0.1~0.8mm / s, the extrusion outlet temperature is 380℃~460℃, and the ingot is extruded into the corresponding wheel profile.

[0012] Preferably, the rimming adopts the following scheme: a strip within the room temperature range is used for rimming processing, so that the straight strip is rimmed to obtain the desired rim shape.

[0013] Preferably, the welding adopts the following scheme: resistance welding is used, and the high temperature generated connects the gaps into the whole wheel. After welding is completed, the weld position needs to be microscopically analyzed, and there must be no pores, slag inclusions, cracks, unfused, or undercuts, and the tensile strength of the weld position cannot be less than 0-10% of the body.

[0014] Preferably, the multi-stage heat treatment uses the following scheme: the welded wheel is subjected to solution and aging heat treatment strengthening, the solution temperature is 440℃~480℃, and the wheel is kept at this temperature for 30min~90min before being quenched and cooled to room temperature. Then, the aging treatment is carried out, and a three-stage aging system is adopted: the room temperature is raised to 90℃~130℃ and kept at this temperature for 3~7h, and then the temperature is raised to 140℃~180℃ and kept at this temperature for 3~7h; in the third stage, the wheel is raised to 190℃~250℃ and kept at this temperature for 2~6h.

[0015] The present invention provides a heat-resistant 7 series aluminum alloy containing Mo element and free of coarse grains, and a preparation method thereof, which improves the heat resistance of the aluminum alloy, thereby increasing the recrystallization temperature of the alloy during thermal deformation and reducing the occurrence of coarse recrystallization.

[0016] Compared with the existing technology, the present invention has the following benefits:

[0017] The present invention adds a small amount of transition metal molybdenum (Mo), zirconium (Zr), and scandium (Sc) elements to the existing 7 series components, and forces molybdenum (Mo), zirconium (Zr), and scandium (Sc) elements to solid-dissolve inside the grains during casting. During the homogenization process, molybdenum (Mo) forms AlMo3, Al 12 The dispersed high-temperature strengthening phase of Mo metal compounds improves the heat resistance of the alloy; zirconium (Zr) and scandium (Sc) form nano-Al3 (Sc, Zr) phases, which play a significant role in grain refinement, solid solution strengthening, phase transformation precipitation and organizational structure optimization, and increase the recrystallization temperature, so that the material can reduce the coarse recrystallization phenomenon on the wheel surface during the hot deformation and cold deformation stages and the high-temperature energy storage release process. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Analyze the position of the coarse grain layer in the cross section of the product;

[0019] Figure 2 This is an observation diagram of the microscopic coarse-grained layer at position 1 of the cross section of the product in Example 1;

[0020] Figure 3 This is an observation diagram of the microscopic coarse-grained layer at position 1 of the cross section of the product in Example 2;

[0021] Figure 4 This is the observation picture of the microscopic coarse-grained layer at position 1 of the cross section of the product in Comparative Example 1;

[0022] Figure 5 This is the observation picture of the microscopic coarse-grained layer at position 1 of the cross section of the product in Comparative Example 2;

[0023] Figure 6 This is the characterization diagram of Al3(Sc, Zr) high temperature strengthening phase;

[0024] Figure 7 AlMo3, Al 12 Mo high temperature strengthening phase characterization diagram. DETAILED DESCRIPTION

[0025] The present invention is described in detail below based on specific implementation cases, and the described implementation cases are only a part of the implementation cases of the present invention.

[0026] Example 1

[0027] A heat-resistant 7-series aluminum alloy containing the Mo element, which has the following mass percentages: 6.10% Zn; 2.1% Mg; 2.20% Cu; 0.18% Zr; 0.18% Mo; 0.09% Sc; 0.03% Ti; Fe≤0.15; Si≤0.10, with the balance being Al, and elements not specified being regarded as impurity elements, with a content of less than 0.01%.

[0028] The preparation method comprises the following steps:

[0029] Step 1, smelting and casting treatment: prepare 97.7% aluminum ingots and 99.995% zinc ingots, 99.5% magnesium ingots, 99.99% copper, zirconium, scandium, etc., and smelt the ingredients according to the above-mentioned element mass percentages. Mo must not exceed 10% of the above-mentioned composition range. Then use hydraulic semi-continuous casting rods. First, the melt temperature is maintained within the range of 770℃±5. The aluminum melt needs to be refined, slag-stripped, and the melt is degassed and filtered using rotor online degassing and plate filtration to make the hydrogen content of the melt less than 0.12mL / 100gAl. Use hydraulic semi-continuous casting rods, the ingot cooling rate is 80K / S, the internal inclusions of the ingot are less than 0.1mm, and the diameter of the casting rod is 158mm.

[0030] Step 2, gradient homogenization treatment: the cast rods are subjected to three-stage homogenization, the first stage is kept at 250℃ for 8h, the second stage is kept at 430℃ for 4h, the third stage is kept at 470℃ for 15h, and then cooled to room temperature at a rate of 250±10℃ / h.

[0031] Step three, reverse extrusion: heat the ingot obtained by homogenization treatment in step two to 340°C, use reverse extrusion, and load the material after heating for 4 hours. The temperature of the ingot barrel is 420°C, the extrusion ratio is 60, the extrusion speed is 0.5mm / s, and the aluminum ingot is heated in a direct fire furnace. The extrusion outlet temperature is 460±5°C, and the ingot is extruded into the corresponding wheel-shaped strip.

[0032] Step 4: Rounding: Use a strip within the room temperature range to perform rounding processing, so that the straight strip can be rounded to obtain the desired wheel rim shape.

[0033] Step 5, welding: resistance welding is used to generate high temperature to connect the gaps into the wheel as a whole. After welding is completed, the weld position needs to be microscopically analyzed. There must be no pores, slag inclusions, cracks, unfused, or undercuts, and the tensile strength of the weld position cannot be less than 0-10% of the body.

[0034] Step 6, multi-stage heat treatment: The welded wheels are subjected to solution and aging heat treatment strengthening, with a solution temperature of 450°C, kept at this temperature for 60 minutes, and then quenched and cooled to room temperature. Then, aging treatment is carried out, using a three-stage aging system: heating from room temperature to 110°C and keeping it for 4 hours, then heating to 150°C and keeping it for 6 hours, and then heating to 195°C and keeping it for 3 hours.

[0035] Step 7, surface treatment: Use a machine to grind the surface of the aged wheel to remove surface impurities, make the surface beautiful, and make the rim cross section flat without coarse grain layer ( Figure 2 and Table 2).

[0036] Example 2

[0037] A heat-resistant 7-series aluminum alloy containing the Mo element, which has the following mass percentages: 5.50% Zn; 1.80% Mg; 1.70% Cu; 0.20% Zr; 0.12% Mo; 0.07% Sc; 0.04% Ti; Fe≤0.15%; Si≤0.10%, with the balance being Al, and elements not specified being regarded as impurity elements with a content of less than 0.01%.

[0038] The preparation method comprises the following steps:

[0039] Step 1, smelting and casting treatment: prepare 97.7% aluminum ingots and 99.995% zinc ingots, 99.5% magnesium ingots, 99.99% copper, zirconium, scandium, etc., and smelt the ingredients according to the above-mentioned element mass percentages. Mo must not exceed 10% of the above-mentioned composition range. Then use hydraulic semi-continuous casting rods. First, the melt temperature is maintained within the range of 770℃±5. The aluminum melt needs to be refined, slag-stripped, and the melt is degassed and filtered using rotor online degassing and plate filtration to make the hydrogen content of the melt less than 0.12mL / 100gAl. Use hydraulic semi-continuous casting rods, the ingot cooling rate is 80K / S, the internal inclusions of the ingot are less than 0.1mm, and the diameter of the casting rod is 158mm.

[0040] Step 2, gradient homogenization treatment: the cast rods are subjected to three-stage homogenization, the first stage is kept at 250℃ for 8h, the second stage is kept at 430℃ for 4h, the third stage is kept at 470℃ for 15h, and then cooled to room temperature at a rate of 250±10℃ / h.

[0041] Step three, reverse extrusion: heat the ingot obtained by homogenization treatment in step two to 340°C, use reverse extrusion, and load the material after heating for 4 hours. The temperature of the ingot barrel is 420°C, the extrusion ratio is 60, the extrusion speed is 0.5mm / s, and the aluminum ingot is heated in a direct fire furnace. The extrusion outlet temperature is 460±5°C, and the ingot is extruded into the corresponding wheel-shaped strip.

[0042] Step 4: Rounding: Use a strip within the room temperature range to perform rounding processing, so that the straight strip can be rounded to obtain the desired wheel rim shape.

[0043] Step 5, welding: resistance welding is used to generate high temperature to connect the gaps into the wheel as a whole. After welding is completed, the weld position needs to be microscopically analyzed. There must be no pores, slag inclusions, cracks, unfused, or undercuts, and the tensile strength of the weld position cannot be less than 0-10% of the body.

[0044] Step 6, multi-stage heat treatment: The welded wheels are subjected to solution and aging heat treatment strengthening, with a solution temperature of 450°C, kept at this temperature for 60 minutes, and then quenched and cooled to room temperature. Then, aging treatment is carried out, using a three-stage aging system: heating from room temperature to 110°C and keeping it for 4 hours, then heating to 150°C and keeping it for 6 hours, and then heating to 195°C and keeping it for 3 hours.

[0045] Step 7, surface treatment: Use a machine to grind the surface of the aged wheel to remove surface impurities, make the surface beautiful, and make the rim cross section flat without coarse grain layer ( Figure 3 and Table 2).

[0046] Comparative Example 1

[0047] A 7 series aluminum alloy and a preparation method thereof, wherein the mass percentage content of each element is: 6.10% Zn; 2.1% Mg; 2.20% Cu; 0.09% Zr; 0.10% Mo; 0.08% Sc; 0.03% Ti; Fe≤0.15; Si≤0.10; the balance is Al, and elements not specified are regarded as impurity elements, with a content of less than 0.01%.

[0048] The preparation method comprises the following steps:

[0049] Step 1, smelting and casting treatment: prepare 97.7% aluminum ingots and 99.995% zinc ingots, 99.5% magnesium ingots, 99.99% copper, zirconium, scandium, etc., and smelt the ingredients according to the above-mentioned element mass percentages. Mo must not exceed 10% of the above-mentioned composition range. Then use hydraulic semi-continuous casting rods. First, the melt temperature is maintained within the range of 770℃±5. The aluminum melt needs to be refined, slag-stripped, and the melt is degassed and filtered using rotor online degassing and plate filtration to make the hydrogen content of the melt less than 0.12mL / 100gAl. Use hydraulic semi-continuous casting rods, the ingot cooling rate is 80K / S, the internal inclusions of the ingot are less than 0.1mm, and the diameter of the casting rod is 158mm.

[0050] Step 2: Gradient homogenization treatment: The cast rods are subjected to three-stage homogenization, with the first stage being kept at 250°C for 8 hours, the second stage being kept at 430°C for 4 hours, and the third stage being kept at 470°C for 15 hours, and then cooled to room temperature at a rate of 250±10°C / h.

[0051] Step three, reverse extrusion: heat the ingot obtained by homogenization treatment in step two to 340°C, use reverse extrusion, and load the material after heating for 4 hours. The temperature of the ingot barrel is 420°C, the extrusion ratio is 60, the extrusion speed is 0.5mm / s, and the aluminum ingot is heated in a direct fire furnace. The extrusion outlet temperature is 460±5°C, and the ingot is extruded into the corresponding wheel-shaped strip.

[0052] Step 4: Rounding: Use a strip within the room temperature range to perform rounding processing, so that the straight strip can be rounded to obtain the desired wheel rim shape.

[0053] Step 5, welding: resistance welding is used to generate high temperature to connect the gaps into the wheel as a whole. After welding is completed, the weld position needs to be microscopically analyzed. There must be no pores, slag inclusions, cracks, unfused, or undercuts, and the tensile strength of the weld position cannot be less than 0-10% of the body.

[0054] Step 6, multi-stage heat treatment: The welded wheels are subjected to solution and aging heat treatment strengthening, with a solution temperature of 450°C, kept at this temperature for 60 minutes, and then quenched and cooled to room temperature. Then, aging treatment is carried out, using a three-stage aging system: heating from room temperature to 110°C and keeping it for 4 hours, then heating to 150°C and keeping it for 6 hours, and then heating to 195°C and keeping it for 3 hours.

[0055] Step 7, surface treatment: The aged wheels are machine-grinded to remove surface impurities and make the surface beautiful. The average coarse grain thickness of the rim cross section reaches 100µm ( Figure 4 and Table 2).

[0056] Comparative Example 2

[0057] A 7 series aluminum alloy and a preparation method thereof, wherein the mass percentage content of each element is: 5.50% Zn; 1.80% Mg; 1.70% Cu; 0.08% Zr; 0.06% Mo; 0.10% Sc; 0.04% Ti; Fe≤0.15%; Si≤0.10%; the balance is Al, and elements not specified are regarded as impurity elements, with a content of less than 0.01%.

[0058] The preparation method comprises the following steps:

[0059] Step 1, smelting and casting treatment: prepare 97.7% aluminum ingots and 99.995% zinc ingots, 99.5% magnesium ingots, 99.99% copper, zirconium, scandium, etc., and smelt the ingredients according to the above-mentioned element mass percentages. Mo must not exceed 10% of the above-mentioned composition range. Then use hydraulic semi-continuous casting rods. First, the melt temperature is maintained within the range of 770℃±5. The aluminum melt needs to be refined, slag-stripped, and the melt is degassed and filtered using rotor online degassing and plate filtration to make the hydrogen content of the melt less than 0.12mL / 100gAl. Use hydraulic semi-continuous casting rods, the ingot cooling rate is 80K / S, the internal inclusions of the ingot are less than 0.1mm, and the diameter of the casting rod is 158mm.

[0060] Step 2, reverse extrusion: cut the cast rod after the casting in step 1 into ingots, heat the ingots to 340°C, use reverse extrusion, load the materials after heating for 4 hours, the ingot barrel temperature is 420°C, the extrusion ratio is 60, the extrusion speed is 0.5mm / s, use a direct fire furnace to heat the aluminum ingot, the extrusion outlet temperature is 460±5°C, and extrude the ingot into the corresponding wheel profile.

[0061] Step three, circumference: Use a strip within the room temperature range to perform circumference processing, so that the straight strip can be circumscribed to obtain the desired wheel rim shape.

[0062] Step 4, welding: resistance welding is used to generate high temperature to connect the gaps into the wheel as a whole. After welding is completed, the weld position needs to be microscopically analyzed. There must be no pores, slag inclusions, cracks, unfused, or undercuts, and the tensile strength of the weld position cannot be less than 0-10% of the body.

[0063] Step 5, multi-stage heat treatment: the welded wheels are subjected to solution and aging heat treatment to strengthen, the solution temperature is 450°C, and the wheels are kept warm for 60 minutes before quenching and cooling to room temperature. Then, aging treatment is carried out, using a three-stage aging system: heating from room temperature to 110°C and keeping warm for 4 hours, then heating to 150°C and keeping warm for 6 hours, and then heating to 195°C and keeping warm for 3 hours. Step 6, surface treatment: the aged wheels are machine-grinded to remove surface impurities and make the surface beautiful. The average coarse grain thickness of the rim cross section reaches 240µm ( Figure 5 and Table 2).

[0064] The tensile strength, yield strength and elongation of each embodiment and comparative example were tested, wherein the testing method for tensile strength was GB / T228.1-2021; the testing method for yield strength was GB / T228.1-2021; the testing method for elongation was GB / T228.1-2021, and the specific data were shown in Table 1.

[0065] Table 1 Mechanical test table of wheel products

[0066] .

[0067] Table 2 Examples 1, 2 and Comparative Examples 1, 2 according to Figure 1 The thickness of the coarse-grained layer at each position of the cross section (in μm).

[0068] Table 2 Thickness of coarse-grained layer at each position of the cross section (in μm)

[0069] .

[0070] Figure 6 The Al3(Sc, Zr) high temperature strengthening phase characterization diagram is analyzed and shown in Table 3.

[0071] Table 3 Al3 (Sc, Zr) high temperature strengthening phase analysis

[0072] .

[0073] Figure 7 AlMo3, Al 12 The Mo high temperature strengthening phase characterization diagram is analyzed and shown in Table 4.

[0074] Table 4 AlMo3, Al 12 Mo high temperature strengthening phase analysis table

[0075] .

Claims

1. A method for preparing a heat-resistant 7-series aluminum alloy containing Mo element and free of coarse grains, characterized in that: Including melting and casting treatment, gradient homogenization treatment, reverse extrusion, rounding, welding, multi-stage heat treatment and surface treatment; The aluminum alloy material contains the following element components in percentage by mass: Zn: 5.10-6.50%; Mg: 1.10-2.30%; Cu: 1.10-2.30%; Zr: 0.10-0.25%; Mo: 0.05-0.20%; Sc: 0.05-0.15%; Ti: 0.02-0.04%; Fe≤0.15%; Si≤0.10%; the ratio of Zr / Sc is 2:1-3:1, and the unspecified elements are regarded as impurity elements with a content of less than 0.01%, and the balance is Al. The alloy is used to prepare wheel hubs with a tensile strength of 600MPa-650MPa, a yield strength of 550MPa-600MPa, and an elongation of 10%-14%; Mo, Zr, and Sc elements are forced to dissolve in the grains, and form metal compound dispersed high-temperature strengthening phases AlMo3 and Al in the homogenization process. 12 Mo and Al3 (Sc, Zr), the size of high temperature strengthening phase is 5-20μm when the alloy solidifies normally; The gradient homogenization treatment adopts the following method: a three-stage homogenization process is adopted, the first stage is kept at 200-300°C for 5-10h, the second stage is kept at 400-450°C for 1-5h, the third stage is kept at 450-500°C for 15-30h, and then cooled to room temperature at a rate of 200°C / h-300°C / h; The reverse extrusion adopts the following method: the ingot after homogenization treatment is heated to 320°C to 350°C, reverse extrusion is adopted, the extrusion ratio is 30 to 70, the extrusion outlet temperature is 380°C to 460°C, and the strip for wheel use is extruded.

2. The method for preparing a heat-resistant 7-series aluminum alloy containing Mo element without coarse grains as claimed in claim 1, characterized in that: The smelting and casting process adopts the following method: by accurately controlling the cooling rate of the casting, the ingot cooling rate is 10K / S to 105K / S, and the diameter of the cast rod is controlled in the range of 90mm to 178mm.