A cast aluminum alloy with high thermal conductivity and toughness and a preparation method thereof

Through the combination of Si, Mg, Zn, Fe, Sr and other elements and alternating electromagnetic field casting technology, the problem of improving the thermal conductivity and toughness of aluminum alloys has been solved, the preparation of strong and tough aluminum alloys with high thermal conductivity has been achieved, and the casting performance of aluminum alloys has been improved. and transportation safety.

CN116287882BActive Publication Date: 2024-10-29NINGBO HELI TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310044024.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-29
Publication Date
2024-10-29
Estimated Expiration
2043-01-29

AI Technical Summary

Technical Problem

When improving the performance of existing aluminum alloys, there are problems such as difficulty in increasing the thermal conductivity, difficulty in boron precipitation, poor fluidity due to low silicon content, and large composition differences, and are easily scratched during transportation.

Method used

Using a combination of Si, Mg, Zn, Fe, Sr and other elements, through non-consumable vacuum die-casting and alternating electromagnetic field casting technology, it ensures the high thermal conductivity and high toughness of the alloy and improves the casting performance, reducing the use of magnesium to avoid scratches during transportation hurt.

Benefits of technology

It realizes the preparation of strong and tough aluminum alloy with high thermal conductivity as cast, improves the thermal conductivity, hardness, fatigue strength and wear resistance, ensuring the safety of parts and casting performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of metal materials and processing thereof, and discloses a cast high-thermal-conductivity and tough aluminum alloy and a preparation method thereof. The aluminum alloy comprises the following components: 8.5wt%-9.5wt% of Si, 0.12wt%-0.17wt% of Mg, 0.6wt%-0.95wt% of Zn, 0.35wt%-0.6wt% of Fe, 0.03wt%-0.06wt% of Sr, and the remainder is Al and inevitable impurity elements. The invention adopts Si, Mg, Zn, Fe and Sr, and the remainder is Al and inevitable impurity elements, so as to ensure that the elements adopted in the application are simpler, and silicon, magnesium, iron, zinc and aluminum are modified by strontium. The elements adopted ensure the fluidity of the die-casting alloy, and iron and strontium are used to overcome the sticking of the die. The electromagnetic casting adopted can ensure good fatigue performance and wear resistance of the hardness, and the hardness, fatigue strength and weight loss due to wear are all improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal materials and processing thereof, and more specifically, relates to a cast high thermal conductivity and toughness aluminum alloy and a preparation method thereof. Background Art

[0002] Aluminum and aluminum alloys are known as "green and environmentally friendly engineering materials of the 21st century" due to their excellent properties such as low density, high specific strength, abundant reserves and easy recycling. They have great development prospects in achieving lightweight transportation, thin and small devices, energy conservation and emission reduction, and green development. Existing aluminum alloys have the following problems when used:

[0003] At present, some public patents use boron to improve the performance of aluminum alloys, which cannot be operated in production. After adding boron, the upper alloy needs to be poured out and degassed before use, which has many uncertainties. Whenever magnesium and manganese are added, the thermal conductivity coefficient cannot be increased. Perhaps the determination method is different. The flash method and other methods are about 10% lower, but the flash method is an internationally recognized standard method. Boron precipitation is very difficult in production. The alloy must be divided into two parts, one for thermal conductivity and the other for ordinary alloys. There are also some public patents with very low silicon content and poor fluidity. The composition of this application is very different from that of traditional patents. In addition, the elongation of this application exceeds 12%, and it has the advantages of fewer elements, no Co and rare earth, and low cost.

[0004] Therefore, a cast aluminum alloy with high thermal conductivity and toughness and a preparation method thereof are proposed.

[0005] Among them, the thermal conductivity is characterized in different ways: 24 in the existing technology is equivalent to 165-169 in the test report, 35 is equivalent to 233, and pure aluminum has the highest. Summary of the invention

[0006] The purpose of the present invention is to provide a cast aluminum alloy with high thermal conductivity and toughness and a preparation method thereof, so as to ensure that the elements used in the application are simpler, and silicon, magnesium, iron, zinc, aluminum and strontium are added to the modification; and the elements used ensure the fluidity of the die-casting alloy, silicon, iron and strontium are used to overcome mold sticking, and electromagnetic casting can ensure good fatigue performance and wear resistance of hardness, and the hardness, fatigue strength and weight loss due to wear are all improved. Electromagnetic casting can obtain fine-grained structure and strengthen the solid solution of alloy elements, and at the same time improve the casting performance of high-strength aluminum alloy, and a small amount of magnesium contributes to hardness, so that the parts will not be scratched during transportation, thereby ensuring the safety of the material.

[0007] The technical solution adopted by the present invention is as follows:

[0008] A cast aluminum alloy with high thermal conductivity and toughness comprises the following components: 8.5wt%-9.5wt% Si, 0.12wt%-0.17wt% Mg, 0.6wt%-0.95wt% Zn, 0.35wt%-0.6wt% Fe, 0.03wt%-0.06wt% Sr, and the remainder is Al and inevitable impurity elements.

[0009] Optionally, the Si is 8.5wt%, the Mg is 0.16wt%, the Zn is 0.6wt%-0.95wt%, the Fe is 0.39wt%, and the Sr is 0.03wt%-0.06wt%.

[0010] Optionally, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is carried out according to the following steps:

[0011] Step 1: Clean the raw materials Si, Mg, Zn and Fe, and then place them in the die-casting mold inside the non-consumable vacuum die-casting machine, and then evacuate and fill them with nitrogen for protective smelting;

[0012] Step 2: After 55 minutes of smelting treatment and 5 minutes before the end of degassing, add AlSr10;

[0013] Step 3: After adding AlSr10, take a density block spectrum sample, let it stand for 20 minutes, then take a density block test again, and after the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot;

[0014] Step 4: The metal ingot is repeatedly smelted 5-8 times, and an alternating electromagnetic field is applied to the melt after smelting to achieve casting, and a die-casting process is performed after casting, and cooling is performed to obtain a high thermal conductivity and toughness aluminum alloy in the cast state.

[0015] Optionally, in step 1, the vacuum degree of the die-casting machine is evacuated to -0.12 MPa, nitrogen is filled to -0.6 MPa, and after filling with nitrogen for 2 minutes, the slag is skimmed and the machine is left to stand for 3 minutes.

[0016] Optionally, in step one, a non-consumable vacuum arc gun is used for arc heating and melting, and the non-consumable vacuum arc gun is 2 m away from the raw material.

[0017] Optionally, after the smelting in step three is cooled to room temperature to obtain a metal ingot, the metal ingot is turned over and the next smelting and die-casting is carried out, and the smelting and die-casting are repeated 6 times.

[0018] Optionally, in step 4, electromagnetic pressure is generated on the molten metal due to the interaction of eddy current and magnetic field, thereby achieving forming casting.

[0019] Optionally, the ingots are preheated to 220°C before melting.

[0020] Optionally, after 55 minutes of smelting treatment in step 2, AlSr10 is added to the alloy liquid, smelted and stirred evenly, and then kept warm for 15 minutes before taking density block spectrum samples.

[0021] Optionally, in step three, a density block spectrum sample is taken, and the specification of the sample is 300mm*300mm*3mm.

[0022] The technical effects achieved by the present invention are:

[0023] (1) This scheme adopts Si as 8.5wt%, Mg as 0.16wt%, Zn as 0.6wt%, Fe as 0.39wt%, Sr as 0.04wt%, and the balance is Al and unavoidable impurity elements, ensuring that the elements used in this application are simpler, silicon, magnesium, iron, zinc, aluminum and strontium are added to the modification; and the elements used ensure the fluidity of the die-casting alloy, silicon, and iron and strontium are used to overcome sticking to the mold;

[0024] (2) This scheme applies an alternating electromagnetic field to the melt after smelting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance. Hardness, fatigue strength, and wear loss weight are all improved. Electromagnetic casting can not only obtain fine-grained structure, but also strengthen the solid solution of alloy elements. At the same time, it can improve the casting performance of high-strength aluminum alloy. After casting, die casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the integration of cast state thermal conductivity and high toughness.

[0025] (3) In this scheme, the strength is achieved by zinc, which has a small impact on the thermal conductivity, and silicon modification. A small amount of magnesium contributes to the hardness to prevent the parts from being scratched during transportation, thus ensuring the safety of the material.

[0026] Contents

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the contents required for describing the embodiments are briefly introduced below. Obviously, the contents described below are only some embodiments of the present invention. For ordinary technicians in this field, other contents can be obtained based on these contents without creative work. DETAILED DESCRIPTION

[0028] The following will combine the contents in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0029] The invention provides a cast high thermal conductivity tough aluminum alloy, comprising the following components: 8.5wt% Si, 0.16wt% Mg, 0.6wt% Zn, 0.39wt% Fe, 0.04wt% Sr, and the remainder Al and inevitable impurity elements.

[0030] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0031] Step 1: 8.0wt% Si, 0.16wt% Mg, 0.6wt% Zn and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0032] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0033] Step 2: After 55 minutes of smelting treatment, AlSr10 containing 0.04wt% Sr is added 5 minutes before the end of degassing; the Fe used in the previous step and the AlSr10 containing Sr work together to solve the sticking film problem, and Si greater than 7.5 can ensure the fluidity of the aluminum alloy;

[0034] After 55 minutes of smelting, AlSr10 was added to the alloy liquid for smelting and stirring, and then the density block spectrum sample was taken after keeping the temperature for 15 minutes; the performance of the alloy was tested by taking the density block spectrum sample;

[0035] Step 3: Take a density block spectrum sample after adding AlSr10, and take a density block test after standing for 20 minutes. After the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot; take a density block spectrum sample, the test piece specification is 300mm*300mm*3mm;

[0036] After the smelting is cooled to room temperature to obtain the metal ingot, the metal ingot is turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated 6 times;

[0037] Step 4: The metal ingot is repeatedly smelted 5-8 times, and an alternating electromagnetic field is applied to the melt after smelting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength, and wear loss weight are all improved. Electromagnetic casting can not only obtain fine-grained structure, but also strengthen the solid solution of alloy elements, and at the same time improve the casting performance of high-strength aluminum alloy. After casting, die casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the integration of cast state thermal conductivity and high toughness;

[0038] Moreover, electromagnetic casting generates electromagnetic pressure on the molten metal under the interaction of eddy current and magnetic field, thus achieving forming casting;

[0039] The metal ingot is preheated to 220°C before smelting to facilitate subsequent smelting treatment. Example 2

[0040] The invention provides a cast high thermal conductivity tough aluminum alloy, comprising the following components: 8.5wt% Si, 0.16wt% Mg, 0.8wt% Zn, 0.39wt% Fe, 0.04wt% Sr, and the balance being Al and inevitable impurity elements.

[0041] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0042] Step 1: 8.0wt% Si, 0.16wt% Mg, 0.8wt% Zn and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0043] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0044] Step 2: After 55 minutes of smelting treatment, AlSr10 containing 0.04wt% Sr is added 5 minutes before the end of degassing; the Fe used in the previous step and the AlSr10 containing Sr work together to solve the sticking film problem, and Si greater than 7.5 can ensure the fluidity of the aluminum alloy;

[0045] After 55 minutes of smelting, AlSr10 was added to the alloy liquid for smelting and stirring, and then the density block spectrum sample was taken after keeping the temperature for 15 minutes; the performance of the alloy was tested by taking the density block spectrum sample;

[0046] Step 3: Take a density block spectrum sample after adding AlSr10, and take a density block test after standing for 20 minutes. After the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot; take a density block spectrum sample, the test piece specification is 300mm*300mm*3mm;

[0047] After the smelting is cooled to room temperature to obtain the metal ingot, the metal ingot is turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated 6 times;

[0048] Step 4: The metal ingot is repeatedly smelted 5-8 times, and an alternating electromagnetic field is applied to the melt after smelting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength, and wear loss weight are all improved. Electromagnetic casting can not only obtain fine-grained structure, but also strengthen the solid solution of alloy elements, and at the same time improve the casting performance of high-strength aluminum alloy. After casting, die casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the integration of cast state thermal conductivity and high toughness;

[0049] Moreover, electromagnetic casting generates electromagnetic pressure on the molten metal under the interaction of eddy current and magnetic field, thus achieving forming casting;

[0050] The metal ingot is preheated to 220°C before smelting to facilitate subsequent smelting treatment. Example 3

[0051] The invention provides a cast high thermal conductivity tough aluminum alloy, comprising the following components: 9.2wt% Si, 0.13wt% Mg, 0.95wt% Zn, 0.39wt% Fe, 0.04wt% Sr, and the remainder Al and inevitable impurity elements.

[0052] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0053] Step 1: 8.0wt% Si, 0.16wt% Mg, 0.95wt% Zn and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0054] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0055] Step 2: After 55 minutes of smelting treatment, AlSr10 containing 0.04wt% Sr is added 5 minutes before the end of degassing; the Fe used in the previous step and the AlSr10 containing Sr work together to solve the sticking film problem, and Si greater than 7.5 can ensure the fluidity of the aluminum alloy;

[0056] After 55 minutes of smelting, AlSr10 was added to the alloy liquid for smelting and stirring, and then the density block spectrum sample was taken after keeping the temperature for 15 minutes; the performance of the alloy was tested by taking the density block spectrum sample;

[0057] Step 3: Take a density block spectrum sample after adding AlSr10, and take a density block test after standing for 20 minutes. After the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot; take a density block spectrum sample, the test piece specification is 300mm*300mm*3mm;

[0058] After the smelting is cooled to room temperature to obtain the metal ingot, the metal ingot is turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated 6 times;

[0059] Step 4: The metal ingot is repeatedly smelted 5-8 times, and an alternating electromagnetic field is applied to the melt after smelting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength, and wear loss weight are all improved. Electromagnetic casting can not only obtain fine-grained structure, but also strengthen the solid solution of alloy elements, and at the same time improve the casting performance of high-strength aluminum alloy. After casting, die casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the integration of cast state thermal conductivity and high toughness;

[0060] Moreover, electromagnetic casting generates electromagnetic pressure on the molten metal under the interaction of eddy current and magnetic field, thus achieving forming casting;

[0061] The metal ingot is preheated to 220°C before smelting to facilitate subsequent smelting treatment. Example 4

[0062] The invention provides a cast high thermal conductivity tough aluminum alloy, comprising the following components: 8.5wt% Si, 0.16wt% Mg, 0.8wt% Zn, 0.39wt% Fe, 0.03wt% Sr, and the balance being Al and inevitable impurity elements.

[0063] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0064] Step 1: 8.0wt% Si, 0.16wt% Mg, 0.8wt% Zn and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0065] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0066] Step 2: After 55 minutes of smelting treatment, add AlSr10 with Sr at 0.03wt% 5 minutes before the end of degassing; the Fe used in the previous step and the AlSr10 containing Sr work together to solve the sticking film problem, and Si greater than 7.5 can ensure the fluidity of the aluminum alloy;

[0067] After 55 minutes of smelting, AlSr10 was added to the alloy liquid for smelting and stirring, and then the density block spectrum sample was taken after keeping the temperature for 15 minutes; the performance of the alloy was tested by taking the density block spectrum sample;

[0068] Step 3: Take a density block spectrum sample after adding AlSr10, and take a density block test after standing for 20 minutes. After the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot; take a density block spectrum sample, the test piece specification is 300mm*300mm*3mm;

[0069] After the smelting is cooled to room temperature to obtain the metal ingot, the metal ingot is turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated 6 times;

[0070] Step 4: The metal ingot is repeatedly smelted 5-8 times, and an alternating electromagnetic field is applied to the melt after smelting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength, and wear loss weight are all improved. Electromagnetic casting can not only obtain fine-grained structure, but also strengthen the solid solution of alloy elements, and at the same time improve the casting performance of high-strength aluminum alloy. After casting, die casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the integration of cast state thermal conductivity and high toughness;

[0071] Moreover, electromagnetic casting generates electromagnetic pressure on the molten metal under the interaction of eddy current and magnetic field, thus achieving forming casting;

[0072] The metal ingot is preheated to 220°C before smelting to facilitate subsequent smelting treatment. Example 5

[0073] The invention provides a cast high thermal conductivity tough aluminum alloy, comprising the following components: 8.5wt% Si, 0.16wt% Mg, 0.8wt% Zn, 0.39wt% Fe, 0.05wt% Sr, and the remainder Al and inevitable impurity elements.

[0074] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0075] Step 1: 8.0wt% Si, 0.16wt% Mg, 0.8wt% Zn and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0076] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0077] Step 2: After 55 minutes of smelting treatment, AlSr10 containing 0.05wt% Sr is added 5 minutes before the end of degassing; the Fe used in the previous step and the AlSr10 containing Sr work together to solve the sticking film problem, and Si greater than 7.5 can ensure the fluidity of the aluminum alloy;

[0078] After 55 minutes of smelting, AlSr10 was added to the alloy liquid for smelting and stirring, and then the density block spectrum sample was taken after keeping the temperature for 15 minutes; the performance of the alloy was tested by taking the density block spectrum sample;

[0079] Step 3: Take a density block spectrum sample after adding AlSr10, and take a density block test after standing for 20 minutes. After the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot; take a density block spectrum sample, the test piece specification is 300mm*300mm*3mm;

[0080] After the smelting is cooled to room temperature to obtain the metal ingot, the metal ingot is turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated 6 times;

[0081] Step 4: The metal ingot is repeatedly smelted 5-8 times, and an alternating electromagnetic field is applied to the melt after smelting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength, and wear loss weight are all improved. Electromagnetic casting can not only obtain fine-grained structure, but also strengthen the solid solution of alloy elements, and at the same time improve the casting performance of high-strength aluminum alloy. After casting, die casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the integration of cast state thermal conductivity and high toughness;

[0082] Moreover, electromagnetic casting generates electromagnetic pressure on the molten metal under the interaction of eddy current and magnetic field, thus achieving forming casting;

[0083] The metal ingot is preheated to 220°C before smelting to facilitate subsequent smelting treatment. Example 6

[0084] The invention provides a cast high thermal conductivity and toughness aluminum alloy, comprising the following components: 8.5wt% Si, 0.16wt% Mg, 0.8wt% Zn, 0.39wt% Fe, 0.05wt% Sr, the remainder being Al and inevitable impurity elements, and also comprising 0.30wt% Er.

[0085] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0086] Step 1: 8.0wt% Si, 0.16wt% Mg, 0.8wt% Zn, 0.30wt% Er and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0087] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0088] Step 2: After 55 minutes of smelting treatment, AlSr10 containing 0.05wt% Sr is added 5 minutes before the end of degassing; the Fe used in the previous step and the AlSr10 containing Sr work together to solve the sticking film problem, and Si greater than 7.5 can ensure the fluidity of the aluminum alloy;

[0089] After 55 minutes of smelting, AlSr10 was added to the alloy liquid for smelting and stirring, and then the density block spectrum sample was taken after keeping the temperature for 15 minutes; the performance of the alloy was tested by taking the density block spectrum sample;

[0090] Step 3: Take a density block spectrum sample after adding AlSr10, and take a density block test after standing for 20 minutes. After the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot; take a density block spectrum sample, the test piece specification is 300mm*300mm*3mm;

[0091] After the smelting is cooled to room temperature to obtain the metal ingot, the metal ingot is turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated 6 times;

[0092] Step 4: The metal ingot is repeatedly smelted 5-8 times, and an alternating electromagnetic field is applied to the melt after smelting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength, and wear loss weight are all improved. Electromagnetic casting can not only obtain fine-grained structure, but also strengthen the solid solution of alloy elements, and at the same time improve the casting performance of high-strength aluminum alloy. After casting, die casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the integration of cast state thermal conductivity and high toughness;

[0093] Moreover, electromagnetic casting generates electromagnetic pressure on the molten metal under the interaction of eddy current and magnetic field, thus achieving forming casting;

[0094] The metal ingot is preheated to 220°C before smelting to facilitate subsequent smelting treatment. Example 7

[0095] The invention provides a cast high thermal conductivity and toughness aluminum alloy, comprising the following components: 8.5wt% Si, 0.16wt% Mg, 0.8wt% Zn, 0.39wt% Fe, 0.05wt% Sr, the remainder being Al and inevitable impurity elements, and also comprising 0.35wt% Er and 0.12wt% Zr.

[0096] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0097] Step 1: 8.0wt% Si, 0.16wt% Mg, 0.8wt% Zn, 0.35wt% Er, 0.12wt% Zr and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0098] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0099] Step 2: After 55 minutes of smelting treatment, AlSr10 containing 0.05wt% Sr is added 5 minutes before the end of degassing; the Fe used in the previous step and the AlSr10 containing Sr work together to solve the sticking film problem, and Si greater than 7.5 can ensure the fluidity of the aluminum alloy;

[0100] After 55 minutes of smelting, AlSr10 was added to the alloy liquid for smelting and stirring, and then the density block spectrum sample was taken after keeping the temperature for 15 minutes; the performance of the alloy was tested by taking the density block spectrum sample;

[0101] Step 3: Take a density block spectrum sample after adding AlSr10, and take a density block test after standing for 20 minutes. After the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot; take a density block spectrum sample, the test piece specification is 300mm*300mm*3mm;

[0102] After the smelting is cooled to room temperature to obtain the metal ingot, the metal ingot is turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated 6 times;

[0103] Step 4: The metal ingot is repeatedly smelted 5-8 times, and an alternating electromagnetic field is applied to the melt after smelting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength, and wear loss weight are all improved. Electromagnetic casting can not only obtain fine-grained structure, but also strengthen the solid solution of alloy elements, and at the same time improve the casting performance of high-strength aluminum alloy. After casting, die casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the integration of cast state thermal conductivity and high toughness;

[0104] Moreover, electromagnetic casting generates electromagnetic pressure on the molten metal under the interaction of eddy current and magnetic field, thus achieving forming casting;

[0105] The metal ingot is preheated to 220°C before smelting to facilitate subsequent smelting treatment.

[0106] Comparative Example 1

[0107] The invention provides a cast high thermal conductivity tough aluminum alloy, comprising the following components: 8.5wt% Si, 0.16wt% Mg, 0.39wt% Fe, and the remainder Al and inevitable impurity elements.

[0108] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0109] Step 1: 8.0wt% Si, 0.16wt% Mg and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0110] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0111] Step 2: Smelting treatment for 55 minutes, after smelting treatment for 55 minutes, after cooling to room temperature to obtain metal ingots, the metal ingots are turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated for 6 times;

[0112] Step 4: The metal ingot is repeatedly melted 5-8 times, and an alternating electromagnetic field is applied to the melt after melting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength and wear loss weight are all improved. Electromagnetic casting can obtain fine-grained structure and strengthen the solid solution of alloy elements. At the same time, it can improve the casting performance of high-strength aluminum alloy. After casting, die-casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the combination of cast thermal conductivity and high toughness.

[0113] Comparative Example 2

[0114] The invention provides a cast high thermal conductivity tough aluminum alloy, comprising the following components: 8.5wt% Si, 0.16wt% Mg, 0.39wt% Fe, and the remainder Al and inevitable impurity elements.

[0115] In this embodiment, a method for preparing a cast high thermal conductivity and toughness aluminum alloy is provided, and the preparation method is carried out according to the following steps:

[0116] Step 1: 8.5wt% Si, 0.16wt% Mg and 0.39wt% Fe of the raw materials are cleaned, and then placed in a die-casting mold inside a non-consumable vacuum die-casting machine for die-casting, and the temperature of the die-casting mold is 230-240°C, preferably 235°C, and then vacuumed and filled with nitrogen for protective smelting. After filling with nitrogen, other air is discharged to ensure that it will not react with the active gas to generate impurities during the die-casting process;

[0117] Vacuum the die casting machine to a vacuum degree of -0.12MPa, fill it with nitrogen to -0.6MPa, and after filling it with nitrogen for 2 minutes, skim the slag and let it stand for 3 minutes; use a non-consumable vacuum arc gun for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material. Arc heating and melting can melt the metal to the maximum extent;

[0118] Step 2: Smelting treatment for 55 minutes, after smelting treatment for 55 minutes, after cooling to room temperature to obtain metal ingots, the metal ingots are turned over to ensure that the die casting is more uniform and the quality is improved, and then the next smelting and die casting are carried out, and the smelting and die casting are repeated for 6 times;

[0119] Step 4: The metal ingot is repeatedly melted 5-8 times, and an alternating electromagnetic field is applied to the melt after melting to achieve casting. Electromagnetic casting can ensure good fatigue performance and wear resistance, and the hardness, fatigue strength and wear loss weight are all improved. Electromagnetic casting can obtain fine-grained structure and strengthen the solid solution of alloy elements. At the same time, it can improve the casting performance of high-strength aluminum alloy. After casting, die-casting is performed and cooled to obtain a high thermal conductivity and toughness aluminum alloy in the cast state, realizing the combination of cast thermal conductivity and high toughness.

[0120] According to the national standard GB228-2002, the alloys prepared in Examples 1 to 5 were processed into standard tensile specimens. The specimens were in the shape of round rods, and the axial direction of the round rods was consistent with the extrusion direction. Room temperature tensile tests were performed to test the mechanical properties of each sample. The test results are shown in Table 1.

[0121] Table 1 Mechanical properties test results of each sample

[0122] .

[0123] In summary, in Example 3, Si is 9.2wt%, Mg is 0.13wt%, Zn is 0.95wt%, Fe is 0.39wt%, Sr is 0.04wt%, and the balance is Al and unavoidable impurity elements. The quality of this embodiment is the best, and the tensile strength reaches 280MPA, the yield strength reaches 135MPA, the elongation reaches 12.9%, and the hardness reaches 80HB, realizing the combination of cast thermal conductivity and high toughness.

[0124] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A cast aluminum alloy with high thermal conductivity and toughness, characterized in that: The composition is as follows: 8.5wt% Si, 0.16wt% Mg, 0.6wt%-0.95wt% Zn, 0.39wt% Fe, 0.03wt%-0.06wt% Sr, and the balance is Al and unavoidable impurity elements; The preparation method of the cast high thermal conductivity and toughness aluminum alloy is carried out according to the following steps: Step 1: Clean the raw materials Si, Mg, Zn and Fe, and then place them in the die-casting mold inside the non-consumable vacuum die-casting machine, and then evacuate and fill them with nitrogen for protective smelting; A non-consumable vacuum arc gun is used for arc heating and melting, and the non-consumable vacuum arc gun is 2m away from the raw material; Step 2: After 55 minutes of smelting treatment and 5 minutes before the end of degassing, add AlSr10; After 55 minutes of smelting, AlSr10 was added to the alloy liquid for smelting and stirring, and then the temperature was kept for 15 minutes before taking density block spectrum samples; Step 3: After 20 minutes of rest, take the density block for testing. When the alloy liquid temperature reaches 680 to 685°C, cool it to obtain a metal ingot. After the smelting is cooled to room temperature to obtain a metal ingot, the metal ingot is turned over and the next smelting and die casting is carried out; Step 4: The metal ingot is repeatedly smelted 5-8 times, and after smelting, an alternating electromagnetic field is applied to the melt to achieve electromagnetic casting, and after casting, a die-casting process is performed, and cooling is performed to obtain a high thermal conductivity and toughness aluminum alloy in the cast state.

2. The method for preparing a cast high thermal conductivity and toughness aluminum alloy according to claim 1, characterized in that: The ingots were preheated to 220°C before smelting.

3. The method for preparing a cast high thermal conductivity and toughness aluminum alloy according to claim 1, characterized in that: In step 3, take the density block spectrum sample, the density block specification is 300mm 300mm 3mm.

Citation Information

Patent Citations

  • High-strength, high-toughness and high-thermal-conductivity die-casting aluminum alloy and manufacturing method thereof

    CN114457263A

  • High-thermal-conductivity and high-toughness die-casting aluminum alloy and preparation method thereof

    CN115558825A