Low-cost deoxidation process for converter steelmaking
By using electromagnetic stirring, ultrasonic stirring and dynamic slag-making technology in converter steelmaking, combined with online analysis and vacuum degassing, the problems of high energy consumption and uniform distribution of traditional stirring methods are solved, and efficient deoxygenation and high-quality steel production are achieved.
Patent Information
- Application Number
- CN202410886759.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional mechanical stirring and bottom blowing stirring consume high energy in converter steelmaking, resulting in equipment wear, and it is impossible to ensure the uniform distribution of deoxidant in the molten steel, affecting the deoxidation effect, resulting in low purity of the molten steel, and affecting the physical and mechanical properties of the steel.
Using electromagnetic stirring or ultrasonic stirring technology, combined with dynamic slag-making technology and online analysis technology, the uniform spraying and real-time monitoring of deoxidants can be achieved through automatic addition system and multi-point dropping system to ensure the fluidity and adsorption capacity of the slag, and combined with vacuum degassing Processing, optimize the deoxidation process.
It reduces energy consumption and equipment wear, improves deoxygenation efficiency and molten steel quality, ensures high purity and excellent performance of steel, and meets high standards of industrial requirements.
Smart Images

Figure CN118957193A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steelmaking production, in particular to a low-cost deoxidation process for converter steelmaking. Background Art
[0002] Steelmaking is the process of converting raw materials such as iron ore or scrap steel into steel through a series of chemical reactions and physical treatments. Steel is an iron-carbon alloy with a carbon content of less than 2%. It has excellent mechanical properties and a wide range of industrial applications. Converter steelmaking is the main steelmaking method, which converts iron into steel by blowing oxygen into high-temperature molten iron to remove impurities such as carbon, silicon, and phosphorus. The traditional converter steelmaking process faces many challenges in the deoxidation process.
[0003] Traditional mechanical stirring and bottom blowing stirring can promote the distribution of deoxidizer, but traditional mechanical stirring and bottom blowing stirring have high energy consumption and cause wear to the equipment. The stirring effect is limited and cannot ensure the uniform distribution of deoxidizer in molten steel, affecting the deoxidation effect. At the same time, primary deoxidation alone cannot completely remove impurities in molten steel, resulting in low purity of molten steel and affecting the physical and mechanical properties of steel.
[0004] Therefore, those skilled in the art provide a low-cost deoxidation process for converter steelmaking to solve the problems raised in the above background technology. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a low-cost deoxidation process for converter steelmaking, which solves the problem that both traditional mechanical stirring and bottom blowing stirring can promote the distribution of deoxidizers, but traditional mechanical stirring and bottom blowing stirring have high energy consumption, cause wear to equipment, have limited stirring effect, and cannot ensure uniform distribution of deoxidizers in molten steel, thus affecting the deoxidation effect.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions: A low-cost deoxidation process for converter steelmaking, comprising the following steps:
[0007] S1. The operator transfers the molten iron from the blast furnace to the converter, and then adds scrap steel to adjust the initial molten iron temperature and composition;
[0008] S2, blowing oxygen into the molten iron through an oxygen lance to remove impurities;
[0009] S3, adding lime and slag-forming materials, allowing the generated oxides to combine with the slag-forming materials to form slag with good fluidity;
[0010] S4. Regularly measure the temperature of molten steel and take samples for composition analysis to determine the timing of deoxidation;
[0011] S5. Spray the deoxidizer evenly into the molten steel through the automatic adding system, using the multi-point delivery system or the spraying technology;
[0012] S6. Electromagnetic stirring or ultrasonic stirring is used. Electromagnetic stirring stirs the molten steel by electromagnetic force, and ultrasonic stirring produces cavitation effect in the molten steel by high-frequency ultrasonic waves.
[0013] S7. Use dynamic slag-making technology to adjust the proportion and addition order of slag-making materials according to the composition and temperature of molten steel to ensure the formation of slag with high fluidity and strong adsorption capacity;
[0014] S8. Use laser induced breakdown spectroscopy or inductively coupled plasma spectroscopy to monitor and quickly feedback the composition of molten steel and improve the control of the deoxidation process;
[0015] S9. After deoxidation is completed, the molten steel is poured into a ladle for further processing or casting, and the upper slag is removed to prevent the slag from entering the ladle;
[0016] S10, performing vacuum degassing after deoxidation to purify the molten steel and improve its quality by reducing the gas content in the molten steel;
[0017] S11. Casting the refined molten steel into profiles or plates to complete steelmaking.
[0018] S1 can effectively utilize scrap steel by adding scrap steel, reduce raw material costs, and adjust the initial temperature and composition of molten iron, laying the foundation for subsequent deoxidation and steelmaking processes; S2 can remove impurities to improve the purity of molten steel and improve the performance of steel. At the same time, the oxidation reaction releases heat, which helps to maintain the high temperature of molten iron; S3 The slag with good fluidity can effectively capture and remove impurities, prevent impurities from re-entering the molten steel, and improve the deoxidation efficiency and molten steel quality; S4 monitors the temperature and composition of molten steel in real time to ensure deoxidation at the best time, avoid adding deoxidizer too early or too late, and ensure the deoxidation effect; S5 The uniform spraying of deoxidizer can improve the deoxidation efficiency, ensure that the deoxidizer is fully in contact with the molten steel, reduce the amount of deoxidizer used, and reduce costs; S6 The stirring in S7 can promote the mixing of molten steel and deoxidizer, improve the reaction speed and efficiency of the deoxidizer, improve the uniformity of the molten steel, and enhance the quality of the steel; the dynamic adjustment of slag-making materials in S7 can optimize the performance of the slag, improve the capture and removal efficiency of impurities, and ensure the stability and efficiency of the deoxidation process; the real-time monitoring and rapid feedback in S8 can adjust the process parameters in time, ensure the precise control of the deoxidation process, and improve the quality of the molten steel and the stability of the process; the dumping and removal of slag in S9 can prevent impurities from contaminating the molten steel, ensure the purity of the molten steel in the subsequent treatment and casting process, and improve the quality of the final product; the vacuum degassing in S10 can effectively remove gases such as hydrogen, oxygen, and nitrogen from the molten steel, reduce the porosity defects of the steel, and improve the mechanical properties and durability of the steel.
[0019] Preferably, in S2, the chemical reaction equation involved in the process of removing impurities by blowing oxygen is as follows:
[0020] Carbon oxidation reaction: C+O2→CO2, where C represents carbon, O2 represents oxygen, and CO2 represents carbon dioxide;
[0021] Sulfur oxidation reaction: S+O2→SO2, where S represents sulfur, O2 represents oxygen, and SO2 represents sulfur dioxide;
[0022] Phosphorus oxidation reaction: P+O2→P2O5. Where P represents phosphorus, O2 represents oxygen, and P2O5 represents phosphorus pentoxide;
[0023] Oxidation reaction of silicon: Si+O2→SiO2, where Si represents silicon, O2 represents oxygen, and SiO2 represents silicon dioxide.
[0024] Preferably, in S3, the process in which lime and slag-making materials combine with the generated oxides to form slag with good fluidity involves the following chemical reaction equation:
[0025] Lime reacts with silicon dioxide: CaO+SiO2→CaSiO3, where CaO represents lime, SiO2 represents silicon dioxide, and CaSiO3 represents calcium silicate;
[0026] Lime reacts with phosphorus pentoxide: 3CaO+P2O5→Ca3(PO4)2, where CaO represents lime, P2O5 represents phosphorus pentoxide, and Ca3(PO4)2 represents calcium phosphate;
[0027] Lime reacts with ferrous oxide: CaO+FeO→CaFeO2, where CaO represents lime, FeO represents ferrous oxide, and CaFeO2 represents calcium ferrite;
[0028] Lime reacts with sulfur dioxide: CaO+SO2→CaSO3, where CaO represents lime, SO2 represents sulfur dioxide, and CaSO3 represents calcium sulfite.
[0029] Preferably, in S5, the speed range of electromagnetic stirring is 20 r / min to 80 r / min, the stirring time range of electromagnetic stirring is 5 min to 15 min, the frequency range of ultrasonic stirring is 20 kHz to 40 kHz, and the stirring time range of ultrasonic stirring is 3 min to 10 min.
[0030] Preferably, in S7, the implementation steps of the dynamic slag making technology are:
[0031] S71. During the deoxidation process, the composition and temperature of the molten steel are measured regularly, and the impurity content in the molten steel is monitored by laser induced breakdown spectroscopy or inductively coupled plasma spectroscopy equipment;
[0032] S72. Determine the type and proportion of slag-forming materials according to the measurement results and process requirements to meet the deoxidation requirements under various compositions and temperatures;
[0033] S73. If the silicon content in the molten steel is high, increase the proportion of lime and quartz sand to promote the formation of SiO2 and form a slag with good fluidity; if the phosphorus content in the molten steel is high, increase the proportion of lime and bauxite to promote the formation of P2O5 and its absorption by the slag; if the sulfur content in the molten steel is high, increase the proportion of lime and fluorite to promote the formation of CaSO4 and its absorption by the slag;
[0034] S74, in the high temperature stage, adding slag-forming materials with high melting points to form initial slag, and gradually adding slag-forming materials with low melting points as the temperature of the molten steel decreases;
[0035] S75. Use an automatic adding system and a multi-point delivery system to evenly add slag-forming materials into the molten steel, and stir and mix them through electromagnetic stirring or ultrasonic stirring technology to ensure that the slag-forming materials are fully mixed in the molten steel to form a uniform slag.
[0036] The benefit of S71 is that it can monitor the composition and temperature of molten steel accurately and in real time, providing a scientific basis for the subsequent adjustment of slag-forming materials, and ensuring the efficiency and stability of the deoxidation process; the benefit of S72 is that it can scientifically determine the types and proportions of slag-forming materials, and can make personalized adjustments according to different molten steel compositions and temperatures, improve the deoxidation effect and efficiency, and avoid material waste; the benefit of S73 is that by adjusting the proportion of slag-forming materials in a targeted manner, it can effectively remove different impurities, form a slag with good fluidity, ensure that impurities are fully absorbed, and improve the purity of molten steel; the benefit of S74 is that it gradually adds slag-forming materials with different melting points, which can form suitable slag at different temperature stages, ensure that the slag maintains good fluidity and adsorption capacity during the deoxidation process, and optimize the deoxidation effect; the benefit of S75 is that uniform addition and stirring can ensure that the slag-forming material is in full contact with the molten steel, forming a uniform slag, improving the adsorption and removal efficiency of impurities, and improving the purity and quality of molten steel.
[0037] Preferably, in S8, the algorithm formula of laser induced breakdown spectroscopy is as follows:
[0038] The laser energy density: Where E is the laser energy density, P is the laser energy, and A is the active area of the laser beam;
[0039] The spectral intensity and element concentration: I i =k i ·C i , where I i is the spectral intensity of element i, k i is the correction coefficient associated with element i, C i is the concentration of element i;
[0040] The concentration is calculated as: Among them, I i is the spectral intensity, k i is the correction coefficient and i is the element concentration.
[0041] Preferably, in S8, the algorithm formula of inductively coupled plasma spectroscopy is as follows:
[0042] The spectral intensity and element concentration: I i =a i ·C i +b i , where I i is the spectral intensity of element i, a i is the sensitivity factor of element i, C i is the concentration of element i, b i is the background spectrum intensity;
[0043] The background correction: I i ′=I i -b i , where I i ′ is the spectral intensity after removing the background;
[0044] The concentration is calculated as: Among them, I i is the spectral intensity, a i is the sensitivity factor and i is the element concentration.
[0045] Preferably, in S10, the vacuum pressure range of the vacuum degassing equipment in the vacuum degassing treatment is 1Pa to 100Pa, and the vacuum degassing treatment time range is 10min to 30min.
[0046] The present invention provides a low-cost deoxidation process for converter steelmaking. It has the following beneficial effects:
[0047] 1. The present invention reduces the operation of mechanical parts, reduces energy consumption and equipment wear, and improves the life and reliability of equipment through electromagnetic stirring technology. Ultrasonic stirring significantly enhances the distribution and reaction effect of the deoxidizer through cavitation effect, further improving the deoxidation efficiency and effect. At the same time, dynamic slag making technology adjusts the slag making material in real time according to the state of molten steel to ensure that the slag always has fluidity and adsorption capacity. The new adsorption material can effectively adsorb and remove impurities in molten steel, further improving the quality of molten steel.
[0048] 2. The present invention can monitor the composition of molten steel in real time through online analysis technology, provide rapid feedback, and adjust process parameters in time to ensure precise control of the deoxidation process. The intelligent control system can combine data and artificial intelligence technology to analyze data in real time and dynamically adjust process parameters to improve the stability and efficiency of the deoxidation process.
[0049] 3. The present invention can further reduce the gas content and inclusions in molten steel through vacuum degassing technology, improve the purity and mechanical properties of steel, and the refined molten steel is of high quality. The produced steel has excellent physical and mechanical properties and meets high standards. At the same time, in the final casting stage, through fine control and perfect deoxidation and refining treatment processes, the produced steel has high purity and high performance, and the quality is stable and reliable. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0051] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0052] The present invention is described in detail below in conjunction with the accompanying drawings:
[0053] Embodiment 1:
[0054] Please see attached Figure 1 The embodiment of the present invention provides a low-cost deoxidation process for converter steelmaking, comprising the following steps:
[0055] S1. Operators transfer molten iron from the blast furnace to the converter and add scrap steel to adjust the initial temperature and composition of the molten iron;
[0056] S2. Use an oxygen lance to blow oxygen into the molten iron to remove impurities. The chemical reactions include oxidation of carbon, oxidation of sulfur, oxidation of phosphorus and oxidation of silicon.
[0057] S3, adding lime and conventional slag-making materials to combine the generated oxides with the slag-making materials to form slag with good fluidity, the chemical reactions including reaction of lime with silicon dioxide, reaction of lime with phosphorus pentoxide and reaction of lime with sulfur dioxide;
[0058] S4. Regularly measure the temperature of molten steel and take samples for composition analysis to determine the timing of deoxidation;
[0059] S5, stirring by a mechanical stirring device, and uniformly adding the deoxidizer into the molten steel by a multi-point delivery system;
[0060] S6. Adjust the proportion and order of adding slag-making materials according to the composition and temperature of the molten steel to ensure the formation of slag with high fluidity and adsorption capacity;
[0061] S7. Use laser induced breakdown spectroscopy to monitor the composition of molten steel, achieve rapid feedback, and improve deoxidation process control;
[0062] S8. After deoxidation is completed, the molten steel is poured into a ladle for further processing or casting, and the upper slag is removed;
[0063] S9, after deoxidation, vacuum degassing treatment is performed, the vacuum pressure range is 50Pa, and the treatment time is 20min;
[0064] S10, casting the refined molten steel into a profile or plate to complete the steelmaking process;
[0065] Summary: Example 1 realizes a low-cost deoxidation process through a combination of mechanical stirring and traditional slag-making materials, and uses mechanical stirring to reduce equipment wear. At the same time, the uniform distribution of the deoxidizer is ensured. The combination of dynamic slag-making technology and LIBS online analysis technology ensures the precise control and efficient progress of the deoxidation process. The vacuum degassing treatment further improves the purity of the molten steel.
[0066] Embodiment 2:
[0067] Please see attached Figure 1 The embodiment of the present invention provides a low-cost deoxidation process for converter steelmaking, comprising the following steps:
[0068] S1. Operators transfer molten iron from the blast furnace to the converter and add scrap steel to adjust the initial temperature and composition of the molten iron;
[0069] S2. Use an oxygen lance to blow oxygen into the molten iron to remove impurities. The chemical reactions include oxidation of carbon, oxidation of sulfur, oxidation of phosphorus and oxidation of silicon.
[0070] S3, adding lime and new slag-forming materials to combine the generated oxides with the slag-forming materials to form slag with good fluidity, the chemical reactions include reaction of lime with silicon dioxide, reaction of lime with phosphorus pentoxide and reaction of lime with sulfur dioxide;
[0071] S4. Regularly measure the temperature of molten steel and take samples for composition analysis to determine the timing of deoxidation;
[0072] S5. Stirring is performed by an electromagnetic stirring device, the stirring speed range is 60r / min, the stirring time range is 10min, and the deoxidizer is evenly sprayed into the molten steel by a multi-point delivery system;
[0073] S6. Adjust the proportion and order of adding slag-making materials according to the composition and temperature of the molten steel to ensure the formation of slag with high fluidity and adsorption capacity;
[0074] S7. Use inductively coupled plasma spectroscopy to monitor the composition of molten steel, achieve rapid feedback, and improve deoxidation process control;
[0075] S8. After deoxidation is completed, the molten steel is poured into a ladle for further processing or casting, and the upper slag is removed;
[0076] S9, after deoxidation, vacuum degassing treatment is performed, the vacuum pressure range is 50Pa, and the treatment time is 20min;
[0077] S10, casting the refined molten steel into a profile or plate to complete the steelmaking process;
[0078] Summary: Example 2 realizes an efficient and low-cost deoxidation process through the combination of electromagnetic stirring and new slag-forming materials. The electromagnetic stirring technology reduces the operation and wear of mechanical parts, improves the uniformity of stirring and the reaction efficiency of the deoxidizer, and the new slag-forming material further improves the fluidity and adsorption capacity of the slag. Combined with the ICP-OES online analysis technology, real-time monitoring and rapid adjustment of the deoxidation process are guaranteed. The vacuum degassing treatment improves the purity and quality of the molten steel.
[0079] Embodiment three:
[0080] Please see attached Figure 1 The embodiment of the present invention provides a low-cost deoxidation process for converter steelmaking, comprising the following steps:
[0081] S1. Operators transfer molten iron from the blast furnace to the converter and add scrap steel to adjust the initial temperature and composition of the molten iron;
[0082] S2. Use an oxygen lance to blow oxygen into the molten iron to remove impurities. The chemical reactions include oxidation of carbon, oxidation of sulfur, oxidation of phosphorus and oxidation of silicon.
[0083] S3, adding lime and traditional slag-making materials to combine the generated oxides with the slag-making materials to form slag with good fluidity;
[0084] S4. Regularly measure the temperature of molten steel and take samples for composition analysis to determine the timing of deoxidation;
[0085] S5. Stirring with an ultrasonic stirring device at a frequency interval of 30 kHz and a stirring time interval of 5 minutes, and spraying the chemical deoxidizer evenly into the molten steel by spraying technology;
[0086] S6. Adjust the proportion and order of adding slag-making materials according to the composition and temperature of the molten steel to ensure the formation of slag with high fluidity and adsorption capacity;
[0087] S7. Use laser induced breakdown spectroscopy to monitor the composition of molten steel, achieve rapid feedback, and improve deoxidation process control;
[0088] S8. After deoxidation is completed, the molten steel is poured into a ladle for further processing or casting, and the upper slag is removed;
[0089] S9, after deoxidation, vacuum degassing treatment is performed, the vacuum pressure range is 50Pa, and the treatment time is 20min;
[0090] S10, casting the refined molten steel into a profile or plate to complete the steelmaking process;
[0091] Summary: Example 3 realizes a low-cost deoxidation process through the combination of ultrasonic stirring technology and chemical deoxidizer. Ultrasonic stirring significantly enhances the distribution and reaction effect of the deoxidizer through the cavitation effect, thereby improving the deoxidation efficiency and effect. LIBS online analysis technology ensures real-time monitoring and rapid adjustment of the deoxidation process. Vacuum degassing treatment improves the purity and quality of molten steel.
[0092] Embodiment 4:
[0093] Please see attached Figure 1 The embodiment of the present invention provides a low-cost deoxidation process for converter steelmaking, comprising the following steps:
[0094] S1. Operators transfer molten iron from the blast furnace to the converter and add scrap steel to adjust the initial temperature and composition of the molten iron;
[0095] S2. Use an oxygen lance to blow oxygen into the molten iron to remove impurities; the main chemical reactions include the oxidation of carbon, sulfur, phosphorus and silicon;
[0096] S3, adding lime and traditional slag-making materials to combine the generated oxides with the slag-making materials to form slag with good fluidity;
[0097] S4. Regularly measure the temperature of molten steel and take samples for composition analysis to determine the timing of deoxidation;
[0098] S5, stirring by a manual stirring device and deoxidizing by using a chemical deoxidizer;
[0099] S6. Adjust the proportion and order of adding slag-making materials according to the composition and temperature of the molten steel to ensure the formation of slag with high fluidity and adsorption capacity;
[0100] S7. Use inductively coupled plasma spectroscopy to monitor the composition of molten steel, achieve rapid feedback, and improve deoxidation process control;
[0101] S8. After deoxidation is completed, the molten steel is poured into a ladle for further processing or casting, and the upper slag is removed;
[0102] S9, after deoxidation, vacuum degassing treatment is performed, the vacuum pressure range is 50Pa, and the treatment time is 20min;
[0103] S10, casting the refined molten steel into a profile or plate to complete the steelmaking process;
[0104] Summary: Example 4 achieves a low-cost deoxidation process through a combination of manual stirring and chemical deoxidizers, but manual stirring reduces equipment costs, and ICP-OES online analysis technology ensures real-time monitoring and rapid adjustment of the deoxidation process, and vacuum degassing treatment improves the purity and quality of molten steel.
[0105] Embodiment five:
[0106] Please see attached Figure 1 The embodiment of the present invention provides a low-cost deoxidation process for converter steelmaking, comprising the following steps:
[0107] S1. Operators transfer molten iron from the blast furnace to the converter and add scrap steel to adjust the initial temperature and composition of the molten iron;
[0108] S2. Use an oxygen lance to blow oxygen into the molten iron to remove impurities; the main chemical reactions include the oxidation of carbon, sulfur, phosphorus and silicon;
[0109] S3, adding lime and new slag-forming materials to combine the generated oxides with the slag-forming materials to form slag with good fluidity;
[0110] S4. Regularly measure the temperature of molten steel and take samples for composition analysis to determine the timing of deoxidation;
[0111] S5. Through the intelligent control system, combined with automatic control technology and artificial intelligence algorithm, the stirring parameters are dynamically adjusted, and electromagnetic stirring is used for stirring, and the deoxidizer is evenly sprayed into the molten steel using a multi-point delivery system;
[0112] S6. Adjust the proportion and order of adding slag-making materials according to the composition and temperature of the molten steel to ensure the formation of slag with high fluidity and adsorption capacity;
[0113] S7. Use inductively coupled plasma spectroscopy to monitor the composition of molten steel, achieve rapid feedback, and improve deoxidation process control;
[0114] S8. After deoxidation is completed, the molten steel is poured into a ladle for further processing or casting, and the upper slag is removed;
[0115] S9, after deoxidation, vacuum degassing treatment is performed, the vacuum pressure range is 50Pa, and the treatment time is 20min;
[0116] S10, casting the refined molten steel into a profile or plate to complete the steelmaking process;
[0117] Summary: Example 5 realizes an efficient and low-cost deoxidation process through intelligent stirring and automated control technology. The combination of intelligent control system and artificial intelligence algorithm optimizes stirring parameters and the use of deoxidizer, improves the stability and efficiency of the process, and ICP-OES online analysis technology ensures real-time monitoring and rapid adjustment of the deoxidation process.
[0118] Comparative experiment 1: Comparative experiment of stirring methods;
[0119] Experimental purpose: To compare the differences in deoxidation effect and energy consumption between different stirring methods;
[0120] Experimental steps:
[0121] S1. Prepare molten iron of the same weight and composition, and add the same amount of scrap steel to adjust the temperature and composition;
[0122] S2. Use an oxygen gun to blow oxygen to remove impurities;
[0123] S3, adding the same amount of lime and slag-making materials;
[0124] S4. Regularly measure the temperature of molten steel and take samples for composition analysis;
[0125] S5. Adding and stirring the deoxidizer using mechanical stirring, electromagnetic stirring and ultrasonic stirring techniques respectively;
[0126] S6. Adjust the proportion and order of adding slag-making materials according to the composition and temperature of molten steel;
[0127] S7. Use LIBS technology to monitor the composition of molten steel;
[0128] S8, performing vacuum degassing treatment;
[0129] S9, casting the refined molten steel into profiles or plates;
[0130] Experimental data table:
[0131] parameter Mechanical stirring Electromagnetic stirring Ultrasonic stirring Initial temperature(℃) 1600 1600 1600 Final temperature(℃) 1550 1555 1545 C content (%) 0.03 0.02 0.01 S content (%) 0.02 0.01 0.005 P content (%) 0.03 0.01 0.01 Si content (%) 0.02 0.01 0.005 Energy consumption (kWh) 300 280 310 Slag fluidity good excellent excellent Deoxygenation time (min) 15 10 8
[0132] Comparative experiment 2: Comparative experiment of slag-making materials;
[0133] Experimental purpose: To compare the effects of different slag-making materials on deoxidation effect and slag fluidity;
[0134] Experimental steps:
[0135] S1. Prepare molten iron of the same weight and composition, and add the same amount of scrap steel to adjust the temperature and composition;
[0136] S2. Use an oxygen gun to blow oxygen to remove impurities;
[0137] S3, adding traditional slag-making materials, new slag-making materials and composite slag-making materials respectively;
[0138] S4. Regularly measure the temperature of molten steel and take samples for composition analysis;
[0139] S5. Electromagnetic stirring technology is uniformly used for stirring;
[0140] S6. Adjust the proportion and order of adding slag-making materials according to the composition and temperature of molten steel;
[0141] S7. Use ICP-OES technology to monitor the composition of molten steel;
[0142] S8, performing vacuum degassing treatment;
[0143] S9, casting the refined molten steel into profiles or plates;
[0144] Experimental data table:
[0145]
[0146]
[0147] Comparative experiment 3: Comparative experiment on deoxidizer types and component detection technology;
[0148] Experimental purpose: To compare the performance of different deoxidizers and component detection technologies in terms of deoxidation effect and process control;
[0149] Experimental steps:
[0150] S1. Prepare molten iron of the same weight and composition, and add the same amount of scrap steel to adjust the temperature and composition;
[0151] S2. Use an oxygen gun to blow oxygen to remove impurities;
[0152] S3, adding the same amount of lime and slag-making materials;
[0153] S4. Regularly measure the temperature of molten steel and take samples for composition analysis;
[0154] S5. Use ultrasonic stirring technology for stirring;
[0155] S6. Use chemical deoxidizer and adopt LIBS technology to monitor the composition of molten steel;
[0156] S7. Use new adsorption materials and ICP-OES technology to monitor the composition of molten steel;
[0157] S8, performing vacuum degassing treatment;
[0158] S9, casting the refined molten steel into profiles or plates;
[0159] Experimental data table:
[0160] parameter Chemical deoxidizer + LIBS New adsorption material + ICP-OES Initial temperature(℃) 1600 1600 Final temperature(℃) 1545 1555 C content (%) 0.02 0.01 S content (%) 0.01 0.005 P content (%) 0.02 0.01 Si content (%) 0.01 0.005 Energy consumption (kWh) 310 290 Slag fluidity good excellent Deoxygenation time (min) 10 8
[0161] Experimental data summary:
[0162] Comparative experiment 1: The results of the comparative experiment of different stirring methods show that ultrasonic stirring performs best in deoxidation effect and slag fluidity, but the energy consumption is relatively high, while electromagnetic stirring has excellent comprehensive performance and low energy consumption;
[0163] Comparative experiment 2: The results of the comparative experiment of different slag-making materials show that the new slag-making material has excellent performance in deoxidation effect and slag fluidity, and relatively low energy consumption. The composite slag-making material further optimizes the slag composition while maintaining a good deoxidation effect;
[0164] Comparative experiment three: The comparative experimental results of different deoxidizers and component monitoring technologies show that the combination of new adsorption materials and ICP-OES technology performs well in deoxidation effect, energy consumption and process control, and has obvious advantages.
[0165] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A low-cost deoxidation process for converter steelmaking, characterized in that: The steps include: S1. The operator transfers the molten iron from the blast furnace to the converter, and then adds scrap steel to adjust the initial molten iron temperature and composition; S2, blowing oxygen into the molten iron through an oxygen lance to remove impurities; S3, adding lime and slag-forming materials, allowing the generated oxides to combine with the slag-forming materials to form slag with good fluidity; S4. Regularly measure the temperature of molten steel and take samples for composition analysis to determine the timing of deoxidation; S5. Spray the deoxidizer evenly into the molten steel through the automatic adding system, using the multi-point delivery system or the spraying technology; S6. Electromagnetic stirring or ultrasonic stirring is used. Electromagnetic stirring stirs the molten steel by electromagnetic force, and ultrasonic stirring produces cavitation effect in the molten steel by high-frequency ultrasonic waves. S7. Use dynamic slag-making technology to adjust the proportion and addition order of slag-making materials according to the composition and temperature of molten steel to ensure the formation of slag with high fluidity and strong adsorption capacity; S8. Use laser induced breakdown spectroscopy or inductively coupled plasma spectroscopy to monitor and quickly feedback the composition of molten steel and improve the control of the deoxidation process; S9. After deoxidation is completed, the molten steel is poured into a ladle for further processing or casting, and the upper slag is removed to prevent the slag from entering the ladle; S10, performing vacuum degassing after deoxidation to purify the molten steel and improve its quality by reducing the gas content in the molten steel; S11. Casting the refined molten steel into profiles or plates to complete steelmaking.
2. A low-cost deoxidation process for converter steelmaking according to claim 1, characterized in that: In S2, the chemical reaction equation involved in the process of removing impurities by blowing oxygen is as follows: Carbon oxidation reaction: C+O2→CO2, where C represents carbon, O2 represents oxygen, and CO2 represents carbon dioxide; Sulfur oxidation reaction: S+O2→SO2, where S represents sulfur, O2 represents oxygen, and SO2 represents sulfur dioxide; Phosphorus oxidation reaction: P+O2→P2O5. Where P represents phosphorus, O2 represents oxygen, and P2O5 represents phosphorus pentoxide; Oxidation reaction of silicon: Si+O2→SiO2, where Si represents silicon, O2 represents oxygen, and SiO2 represents silicon dioxide.
3. A low-cost deoxidation process for converter steelmaking according to claim 1, characterized in that: In S3, the process in which lime and slag-making materials combine with the generated oxides to form a slag with good fluidity involves the following chemical reaction equation: Lime reacts with silicon dioxide: CaO+SiO2→CaSiO3, where CaO represents lime, SiO2 represents silicon dioxide, and CaSiO3 represents calcium silicate; Lime reacts with phosphorus pentoxide: 3CaO+P2O5→Ca3(PO4)2, where CaO represents lime, P2O5 represents phosphorus pentoxide, and Ca3(PO4)2 represents calcium phosphate; Lime reacts with ferrous oxide: CaO+FeO→CaFeO2, where CaO represents lime, FeO represents ferrous oxide, and CaFeO2 represents calcium ferrite; Lime reacts with sulfur dioxide: CaO+SO2→CaSO3, where CaO represents lime, SO2 represents sulfur dioxide, and CaSO3 represents calcium sulfite.
4. A low-cost deoxidation process for converter steelmaking according to claim 1, characterized in that: In S5, the speed range of electromagnetic stirring is 20 r / min to 80 r / min, the stirring time range of electromagnetic stirring is 5 min to 15 min, the frequency range of ultrasonic stirring is 20 kHz to 40 kHz, and the stirring time range of ultrasonic stirring is 3 min to 10 min.
5. A low-cost deoxidation process for converter steelmaking according to claim 1, characterized in that: In S7, the implementation steps of the dynamic slag making technology are: S71. During the deoxidation process, the composition and temperature of the molten steel are measured regularly, and the impurity content in the molten steel is monitored by laser induced breakdown spectroscopy or inductively coupled plasma spectroscopy equipment; S72. Determine the type and proportion of slag-forming materials according to the measurement results and process requirements to meet the deoxidation requirements under various compositions and temperatures; S73. If the silicon content in the molten steel is high, increase the proportion of lime and quartz sand to promote the formation of SiO2 and form a slag with good fluidity; if the phosphorus content in the molten steel is high, increase the proportion of lime and bauxite to promote the formation of P2O5 and its absorption by the slag; if the sulfur content in the molten steel is high, increase the proportion of lime and fluorite to promote the formation of CaSO4 and its absorption by the slag; S74, in the high temperature stage, adding slag-forming materials with high melting points to form initial slag, and gradually adding slag-forming materials with low melting points as the temperature of the molten steel decreases; S75. Use an automatic adding system and a multi-point delivery system to evenly add slag-forming materials into the molten steel, and stir and mix them through electromagnetic stirring or ultrasonic stirring technology to ensure that the slag-forming materials are fully mixed in the molten steel to form a uniform slag.
6. A low-cost deoxidation process for converter steelmaking according to claim 1, characterized in that: In S8, the algorithm formula of laser induced breakdown spectroscopy is as follows: The laser energy density: Where E is the laser energy density, P is the laser energy, and A is the active area of the laser beam; The spectral intensity and element concentration: I i =k i ·C i , where I i is the spectral intensity of element i, k i is the correction coefficient associated with element i, C i is the concentration of element i; The concentration is calculated as: Among them, I i is the spectral intensity, k i is the correction coefficient and i is the element concentration.
7. A low-cost deoxidation process for converter steelmaking according to claim 1, characterized in that: In S8, the algorithm formula of inductively coupled plasma spectrum is as follows: The spectral intensity and element concentration: I i =a i ·C i +b i , where I i is the spectral intensity of element i, a i is the sensitivity factor of element i, C i is the concentration of element i, b i is the background spectrum intensity; The background correction: I i ′=I i -b i , where I i ′ is the spectral intensity after removing the background; The concentration is calculated as: Among them, I i is the spectral intensity, a i is the sensitivity factor and i is the element concentration.
8. A low-cost deoxidation process for converter steelmaking according to claim 1, characterized in that: In the above S10, the vacuum pressure range of the vacuum degassing equipment in the vacuum degassing treatment is 1Pa to 100Pa, and the vacuum degassing treatment time range is 10min to 30min.
Citation Information
Cited By
Liquid zinc detection method based on LIBS (laser-induced breakdown spectroscopy) technology
CN119555669A
Method for producing low-oxygen steel by adopting electromagnetic stirring system in 150t converter
CN121227967A