A lightweight high-pressure resistant aluminum alloy material and a preparation method thereof

By introducing pretreated high-pressure resistant aerogel particles into aluminum alloy materials, the problem of lightweight and high-strength aluminum alloy materials has been solved, realizing the preparation of lightweight high-pressure resistant aluminum alloys and meeting the lightweight requirements of portable electronic products and transportation vehicles.

CN116287892BActive Publication Date: 2024-11-22苏州创泰合金材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211680178.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-11-22
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

Existing aluminum alloy materials cannot simultaneously achieve lightweight, high strength, and high compressive strength in portable electronic products and transportation vehicles, thus failing to meet the demands for thinness and lightness.

Method used

A lightweight, high-pressure resistant aluminum alloy material is prepared by combining pretreated high-pressure resistant aerogel particles with an aluminum alloy substrate. The aerogel particles have high porosity and high hardness, which enhances the mechanical properties of the material.

Benefits of technology

It achieves lightweighting and improved compressive strength of aluminum alloy materials, meeting the requirements of portable electronic products and vehicles for high decorative and mechanical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a lightweight high-pressure resistant aluminum alloy material and a preparation method thereof. The preparation steps are as follows: S1: melt the aluminum alloy substrate, add pretreated high-pressure resistant aerogel particles, and stir at a rotation speed of 80-100rpm for 20min; S2: increase the stirring speed, stir at a rotation speed of 300-400rpm for 10-20min; S3: cast into a mold, and cool naturally in the air. The lightweight high-pressure resistant aluminum alloy material of the present invention adopts high-pressure resistant aerogel particles, and the aerogel particles have the characteristics of large porosity and low density, which can greatly reduce the weight of the material and achieve the effect of lightness. At the same time, the aerogel used is silicon carbide aerogel, which has the characteristics of high hardness, and can improve the mechanical strength of the aerogel itself, thereby improving the mechanical effects such as the compressive strength of the aluminum alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of alloy materials, and in particular to a lightweight, high-pressure-resistant aluminum alloy material and a preparation method thereof. Background Art

[0002] With the development of lightweight portable electronic products and lightweight transportation vehicles, higher requirements are also put forward for the performance of aluminum alloy materials. For example, with the development of large-screen and lightweight portable electronic products such as tablet computers, laptops, and smart phones, there is an urgent need for lightweight and high-strength aluminum alloy shells to improve the body's compression and bending resistance to avoid bending and bending of the body, while also meeting the high decorative requirements of portable electronic products for appearance parts. For another example, with the lightweight development of transportation vehicles such as automobiles, trucks, and rail vehicles, the body's bumpers, anti-collision beams, pillow beams, cross beams, etc. are in urgent need of lightweight and high-strength aluminum alloys with excellent performance to replace existing steel materials, so as to achieve the purpose of lightweight body structure and energy conservation and emission reduction. Therefore, reducing the weight of aluminum alloys without affecting their mechanical properties, or even improving their mechanical properties, has become one of the main problems that need to be studied and solved at present. Summary of the invention

[0003] Technical problem to be solved: The purpose of the present invention is to provide a lightweight, high-pressure resistant aluminum alloy material and a preparation method thereof. By adopting high-pressure resistant aerogel particles, the aerogel particles have the characteristics of large porosity and low density, which can greatly reduce the weight of the material and achieve a lightweight effect. At the same time, the aerogel used is silicon carbide aerogel, which has the characteristics of high hardness, and can improve the mechanical strength of the aerogel itself, thereby improving the compressive strength and other mechanical effects of the aluminum alloy.

[0004] Technical solution: A lightweight high-pressure resistant aluminum alloy material, which is composited by pretreated high-pressure resistant aerogel particles and an aluminum alloy substrate, wherein the aluminum alloy substrate includes the following components:

[0005] Si is 0.2-1.0%;

[0006] Mg: 0.5-1.5%;

[0007] Zn: 0.2- 0.5%;

[0008] Ce: 0.2-0.35%

[0009] The balance is Al.

[0010] The method for preparing the above-mentioned lightweight high-pressure resistant aluminum alloy material is characterized in that the preparation steps are as follows:

[0011] S1: Melt the aluminum alloy substrate, add the pretreated high-pressure resistant aerogel particles, and stir at a speed of 80-100 rpm for 20 minutes;

[0012] S2: Increase the stirring speed and stir at 300-400 rpm for 10-20 min;

[0013] S3: Cast into a mold and cool naturally in the air.

[0014] Preferably, the addition amount of the pretreated high pressure resistant aerogel particles is 5.0-13.0% of the aluminum alloy substrate.

[0015] Preferably, the particle size of the high pressure resistant aerogel particles is 0.05-0.1 μm.

[0016] Preferably, the preparation method of the high pressure resistant aerogel particles is as follows:

[0017] S11: mixing the brucite fiber dispersion and the silica sol and stirring evenly, adding the konjac glucomannan aqueous solution and stirring evenly to obtain a wet gel;

[0018] S12: freezing the wet gel to obtain a frozen block gel;

[0019] S13: vacuum drying the block gel to obtain a porous composite gel;

[0020] S14: sintering the porous composite gel at a high temperature of 700-800° C., and crushing the porous composite gel to obtain high-pressure resistant aerogel particles.

[0021] Preferably, the mass fraction of brucite fiber in the brucite fiber dispersion is 10-20%; and the length of the brucite fiber is 0.1-2.0 μm.

[0022] Preferably, the content of konjac glucomannan in the konjac glucomannan aqueous solution is 15-22 wt.%.

[0023] Preferably, the volume ratio of the brucite fiber dispersion, silica sol and konjac glucomannan aqueous solution is (5-10):100:(10-25).

[0024] Preferably, the pretreatment method of the pretreated high pressure resistant aerogel particles is:

[0025] Step 1: Dissolve 13 parts of magnesium nitrate hexahydrate and 6 parts of sodium carbonate in 50 parts of water to obtain a magnesium nitrate solution and a sodium carbonate solution;

[0026] Step 2: Place 40 parts of high pressure resistant aerogel particles in a magnesium nitrate solution, add a sodium carbonate solution, and stir and mix thoroughly;

[0027] Step 3: Aging for 3 hours, filtering the precipitate, washing it thoroughly with distilled water, and then washing it with ethanol;

[0028] Step 4: Place in an oven at 80°C for 4 hours and then calcine at 600°C for 3 hours. Beneficial Effects

[0029] The present invention adopts high-pressure resistant aerogel particles, which have the characteristics of large porosity and low density, and can greatly reduce the weight of the material to achieve a lightweight effect.

[0030] The aerogel used in the present invention is silicon carbide aerogel, which has the characteristics of high hardness and can improve the mechanical strength of the aerogel itself, thereby improving the compressive strength and other mechanical effects of the aluminum alloy.

[0031] The present invention also uses konjac glucomannan as a supporting skeleton, which can further maintain the shape of the aerogel and reduce the disadvantage of collapse during the freezing molding process.

[0032] In the high-pressure resistant aerogel particles of the present invention, silicon does not have a strong adsorption effect like magnesium and is not a surface active element. Therefore, brucite fiber is added in the present application, which can not only improve the mechanical energy absorption of the aerogel, but also improve the bonding performance with the alloy.

[0033] The invention pre-treats the high-pressure resistant aerogel particles and attaches nano-magnesium oxide, thereby improving the bonding ability between the aluminum alloy and the high-pressure resistant aerogel particles. DETAILED DESCRIPTION

[0034] The present invention proposes a lightweight high-pressure resistant aluminum alloy material and a preparation method thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention will be further described in detail with reference to the embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Example 1

[0035] The preparation method of the pretreated high pressure resistant aerogel particles is as follows:

[0036] Step 1: Mixing a 10% mass fraction brucite fiber dispersion with silica sol and stirring evenly, adding a 15wt.% konjac glucomannan aqueous solution and stirring evenly to obtain a wet gel; the brucite fiber has a length of 0.1-2.0 μm; and the volume ratio of the brucite fiber dispersion, silica sol and konjac glucomannan aqueous solution is 5:100:10;

[0037] Step 2: Freezing the wet gel to obtain a frozen block gel;

[0038] Step 3: vacuum drying the block gel to obtain a porous composite gel;

[0039] Step 4: The porous composite gel is subjected to high-temperature sintering at a sintering temperature of 700° C., and after crushing, high-pressure resistant aerogel particles with a particle size of 0.05-0.1 μm are obtained.

[0040] Step 5: Dissolve 13 parts of magnesium nitrate hexahydrate and 6 parts of sodium carbonate in 50 parts of water to obtain a magnesium nitrate solution and a sodium carbonate solution;

[0041] Step 6: Place 40 parts of high pressure resistant aerogel particles in a magnesium nitrate solution, add a sodium carbonate solution, and stir and mix thoroughly;

[0042] Step 7: Aging for 3 hours, filtering the precipitate, washing it thoroughly with distilled water, and then washing it with ethanol;

[0043] Step 8: Place in an oven at 80°C for 4 hours and then calcine at 600°C for 3 hours. Example 2

[0044] The preparation method of the pretreated high pressure resistant aerogel particles is as follows:

[0045] Step 1: Mixing a 10% mass fraction brucite fiber dispersion with silica sol and stirring evenly, adding a 17wt.% konjac glucomannan aqueous solution and stirring evenly to obtain a wet gel; the length of the brucite fiber is 0.1-2.0 μm; the volume ratio of the brucite fiber dispersion, silica sol and konjac glucomannan aqueous solution is 6:100:14;

[0046] Step 2: Freezing the wet gel to obtain a frozen block gel;

[0047] Step 3: vacuum drying the block gel to obtain a porous composite gel;

[0048] Step 4: The porous composite gel is subjected to high-temperature sintering at a sintering temperature of 700° C., and after crushing, high-pressure resistant aerogel particles with a particle size of 0.05-0.1 μm are obtained.

[0049] Step 5: Dissolve 13 parts of magnesium nitrate hexahydrate and 6 parts of sodium carbonate in 50 parts of water to obtain a magnesium nitrate solution and a sodium carbonate solution;

[0050] Step 6: Place 40 parts of high pressure resistant aerogel particles in a magnesium nitrate solution, add a sodium carbonate solution, and stir and mix thoroughly;

[0051] Step 7: Aging for 3 hours, filtering the precipitate, washing it thoroughly with distilled water, and then washing it with ethanol;

[0052] Step 8: Place in an oven at 80°C for 4 hours and then calcine at 600°C for 3 hours. Example 3

[0053] The preparation method of the pretreated high pressure resistant aerogel particles is as follows:

[0054] Step 1: Mixing a 15% mass fraction brucite fiber dispersion with silica sol and stirring evenly, adding a 18wt.% konjac glucomannan aqueous solution and stirring evenly to obtain a wet gel; the length of the brucite fiber is 0.1-2.0 μm; the volume ratio of the brucite fiber dispersion, silica sol and konjac glucomannan aqueous solution is 7:100:18;

[0055] Step 2: Freezing the wet gel to obtain a frozen block gel;

[0056] Step 3: vacuum drying the block gel to obtain a porous composite gel;

[0057] Step 4: The porous composite gel is subjected to high temperature sintering at a sintering temperature of 750° C. and crushed to obtain high pressure resistant aerogel particles with a particle size of 0.05-0.1 μm.

[0058] Step 5: Dissolve 13 parts of magnesium nitrate hexahydrate and 6 parts of sodium carbonate in 50 parts of water to obtain a magnesium nitrate solution and a sodium carbonate solution;

[0059] Step 6: Place 40 parts of high pressure resistant aerogel particles in a magnesium nitrate solution, add a sodium carbonate solution, and stir and mix thoroughly;

[0060] Step 7: Aging for 3 hours, filtering the precipitate, washing it thoroughly with distilled water, and then washing it with ethanol;

[0061] Step 8: Place in an oven at 80°C for 4 hours and then calcine at 600°C for 3 hours. Example 4

[0062] The preparation method of the pretreated high pressure resistant aerogel particles is as follows:

[0063] Step 1: Mixing a 15% mass fraction brucite fiber dispersion with silica sol and stirring evenly, adding a 19wt.% konjac glucomannan aqueous solution and stirring evenly to obtain a wet gel; the length of the brucite fiber is 0.1-2.0 μm; the volume ratio of the brucite fiber dispersion, silica sol and konjac glucomannan aqueous solution is 8:100:20;

[0064] Step 2: Freezing the wet gel to obtain a frozen block gel;

[0065] Step 3: vacuum drying the block gel to obtain a porous composite gel;

[0066] Step 4: The porous composite gel is subjected to high temperature sintering at a sintering temperature of 750° C. and crushed to obtain high pressure resistant aerogel particles with a particle size of 0.05-0.1 μm.

[0067] Step 5: Dissolve 13 parts of magnesium nitrate hexahydrate and 6 parts of sodium carbonate in 50 parts of water to obtain a magnesium nitrate solution and a sodium carbonate solution;

[0068] Step 6: Place 40 parts of high pressure resistant aerogel particles in a magnesium nitrate solution, add a sodium carbonate solution, and stir and mix thoroughly;

[0069] Step 7: Aging for 3 hours, filtering the precipitate, washing it thoroughly with distilled water, and then washing it with ethanol;

[0070] Step 8: Place in an oven at 80°C for 4 hours and then calcine at 600°C for 3 hours. Example 5

[0071] The preparation method of the pretreated high pressure resistant aerogel particles is as follows:

[0072] Step 1: Mixing a 20% mass fraction brucite fiber dispersion with silica sol and stirring evenly, adding a 20wt.% konjac glucomannan aqueous solution and stirring evenly to obtain a wet gel; the length of the brucite fiber is 0.1-2.0 μm; the volume ratio of the brucite fiber dispersion, silica sol and konjac glucomannan aqueous solution is 9:100:23;

[0073] Step 2: Freezing the wet gel to obtain a frozen block gel;

[0074] Step 3: vacuum drying the block gel to obtain a porous composite gel;

[0075] Step 4: The porous composite gel is subjected to high temperature sintering at a sintering temperature of 800° C. After crushing, high pressure resistant aerogel particles with a particle size of 0.05-0.1 μm are obtained.

[0076] Step 5: Dissolve 13 parts of magnesium nitrate hexahydrate and 6 parts of sodium carbonate in 50 parts of water to obtain a magnesium nitrate solution and a sodium carbonate solution;

[0077] Step 6: Place 40 parts of high pressure resistant aerogel particles in a magnesium nitrate solution, add a sodium carbonate solution, and stir and mix thoroughly;

[0078] Step 7: Aging for 3 hours, filtering the precipitate, washing it thoroughly with distilled water, and then washing it with ethanol;

[0079] Step 8: Place in an oven at 80°C for 4 hours and then calcine at 600°C for 3 hours. Example 6

[0080] The preparation method of the pretreated high pressure resistant aerogel particles is as follows:

[0081] Step 1: Mixing a 20% mass fraction brucite fiber dispersion with silica sol and stirring evenly, adding a 22wt.% konjac glucomannan aqueous solution and stirring evenly to obtain a wet gel; the length of the brucite fiber is 0.1-2.0 μm; the volume ratio of the brucite fiber dispersion, silica sol and konjac glucomannan aqueous solution is 10:100:25;

[0082] Step 2: Freezing the wet gel to obtain a frozen block gel;

[0083] Step 3: vacuum drying the block gel to obtain a porous composite gel;

[0084] Step 4: The porous composite gel is subjected to high temperature sintering at a sintering temperature of 800° C. After crushing, high pressure resistant aerogel particles with a particle size of 0.05-0.1 μm are obtained.

[0085] Step 5: Dissolve 13 parts of magnesium nitrate hexahydrate and 6 parts of sodium carbonate in 50 parts of water to obtain a magnesium nitrate solution and a sodium carbonate solution;

[0086] Step 6: Place 40 parts of high pressure resistant aerogel particles in a magnesium nitrate solution, add a sodium carbonate solution, and stir and mix thoroughly;

[0087] Step 7: Aging for 3 hours, filtering the precipitate, washing it thoroughly with distilled water, and then washing it with ethanol;

[0088] Step 8: Place in an oven at 80°C for 4 hours and then calcine at 600°C for 3 hours. Example 7

[0089] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0090] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 5, and stirring at a rotation speed of 80 rpm for 20 min; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 5.0% of the aluminum alloy substrate;

[0091] S2: Increase the stirring speed and stir at 300 rpm for 10 min;

[0092] S3: Cast into a mold and cool naturally in the air.

[0093] The aluminum alloy substrate comprises the following components:

[0094] Si is 0.2%;

[0095] Mg: 0.5%;

[0096] Zn: 0.2%;

[0097] Ce: 0.2%

[0098] The balance is Al. Example 8

[0099] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0100] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 5, and stirring at a rotation speed of 85 rpm for 20 min; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 7.0% of the aluminum alloy substrate;

[0101] S2: Increase the stirring speed and stir at 300 rpm for 15 min;

[0102] S3: Cast into a mold and cool naturally in the air.

[0103] The aluminum alloy substrate comprises the following components:

[0104] Si is 0.4%;

[0105] Mg: 0.8%;

[0106] Zn: 0.3%;

[0107] Ce: 0.25%

[0108] The balance is Al. Example 9

[0109] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0110] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 5, and stirring at a rotation speed of 90 rpm for 20 minutes; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 9.0% of the aluminum alloy substrate;

[0111] S2: Increase the stirring speed and stir at 350 rpm for 15 min;

[0112] S3: Cast into a mold and cool naturally in the air.

[0113] The aluminum alloy substrate comprises the following components:

[0114] Si is 0.6%;

[0115] Mg: 1.0%;

[0116] Zn: 0.4%;

[0117] Ce: 0.25%

[0118] The balance is Al. Example 10

[0119] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0120] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 5, and stirring at a rotation speed of 95 rpm for 20 min; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 11.0% of the aluminum alloy substrate;

[0121] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0122] S3: Cast into a mold and cool naturally in the air.

[0123] The aluminum alloy substrate comprises the following components:

[0124] Si is 0.8%;

[0125] Mg: 1.0%;

[0126] Zn: 0.4%;

[0127] Ce: 0.3%

[0128] The balance is Al. Embodiment 11

[0129] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0130] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 5, and stirring at a rotation speed of 100 rpm for 20 minutes; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 13.0% of the aluminum alloy substrate;

[0131] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0132] S3: Cast into a mold and cool naturally in the air.

[0133] The aluminum alloy substrate comprises the following components:

[0134] Si is 1.0%;

[0135] Mg: 1.5%;

[0136] Zn: 0.5%;

[0137] Ce: 0.35%

[0138] The balance is Al. Example 12

[0139] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0140] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 1, and stirring at a rotation speed of 95 rpm for 20 minutes; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 11.0% of the aluminum alloy substrate;

[0141] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0142] S3: Cast into a mold and cool naturally in the air.

[0143] The aluminum alloy substrate comprises the following components:

[0144] Si is 0.8%;

[0145] Mg: 1.0%;

[0146] Zn: 0.4%;

[0147] Ce: 0.3%

[0148] The balance is Al. Embodiment 13

[0149] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0150] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 2, and stirring at a rotation speed of 95 rpm for 20 min; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 11.0% of the aluminum alloy substrate;

[0151] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0152] S3: Cast into a mold and cool naturally in the air.

[0153] The aluminum alloy substrate comprises the following components:

[0154] Si is 0.8%;

[0155] Mg: 1.0%;

[0156] Zn: 0.4%;

[0157] Ce: 0.3%

[0158] The balance is Al. Embodiment 14

[0159] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0160] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 3, and stirring at a rotation speed of 95 rpm for 20 min; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 11.0% of the aluminum alloy substrate;

[0161] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0162] S3: Cast into a mold and cool naturally in the air.

[0163] The aluminum alloy substrate comprises the following components:

[0164] Si is 0.8%;

[0165] Mg: 1.0%;

[0166] Zn: 0.4%;

[0167] Ce: 0.3%

[0168] The balance is Al. Embodiment 15

[0169] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0170] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 4, and stirring at a rotation speed of 95 rpm for 20 min; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 11.0% of the aluminum alloy substrate;

[0171] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0172] S3: Cast into a mold and cool naturally in the air.

[0173] The aluminum alloy substrate comprises the following components:

[0174] Si is 0.8%;

[0175] Mg: 1.0%;

[0176] Zn: 0.4%;

[0177] Ce: 0.3%

[0178] The balance is Al. Example 16

[0179] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0180] S1: Melting the aluminum alloy substrate, adding the pretreated high-pressure resistant aerogel particles of Example 6, and stirring at a rotation speed of 95 rpm for 20 min; wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 11.0% of the aluminum alloy substrate;

[0181] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0182] S3: Cast into a mold and cool naturally in the air.

[0183] The aluminum alloy substrate comprises the following components:

[0184] Si is 0.8%;

[0185] Mg: 1.0%;

[0186] Zn: 0.4%;

[0187] Ce: 0.3%

[0188] The balance is Al. Comparative Example 1

[0189] The difference between this comparative example and Example 10 is that unpretreated high pressure resistant aerogel particles are used, specifically:

[0190] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0191] S1: Melting the aluminum alloy substrate, adding the high pressure aerogel particles of Example 5, and stirring at a rotation speed of 95 rpm for 20 min; wherein the amount of the high pressure aerogel particles added is 11.0% of the aluminum alloy substrate;

[0192] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0193] S3: Cast into a mold and cool naturally in the air.

[0194] The aluminum alloy substrate comprises the following components:

[0195] Si is 0.8%;

[0196] Mg: 1.0%;

[0197] Zn: 0.4%;

[0198] Ce: 0.3%

[0199] The balance is Al. Comparative Example 2

[0200] The difference between this comparative example and Example 10 is that no pre-treated high pressure resistant aerogel particles are used. Specifically:

[0201] A method for preparing a lightweight high-pressure resistant aluminum alloy material, characterized in that the preparation steps are as follows:

[0202] S1: Melt the aluminum alloy substrate and stir at a speed of 95 rpm for 20 min;

[0203] S2: Increase the stirring speed and stir at 400 rpm for 20 min;

[0204] S3: Cast into a mold and cool naturally in the air.

[0205] The aluminum alloy substrate comprises the following components:

[0206] Si is 0.8%;

[0207] Mg: 1.0%;

[0208] Zn: 0.4%;

[0209] Ce: 0.3%

[0210] The balance is Al.

[0211] According to the national standard GB / T16865-2013, the lightweight high-pressure aluminum alloy material of each embodiment is processed into a standard tensile specimen, and stretched at room temperature on a DNS200 electronic tensile testing machine. The stretching rate is 2 mm / min. Three groups of data are measured for each sample, and the average value is taken. The mechanical properties are shown in Table 1.

[0212] Table 1 Characterization of mechanical properties of aluminum alloy materials in various examples

[0213] Tensile strength (MPa) Yield strength (MPa) Elongation (%) Example 7 537.6 457.6 16.3 Example 8 545.8 472.3 16.7 Example 9 561.9 489.5 17.1 Example 10 587.4 497.1 17.4 Embodiment 11 592.1 499.3 17.3 Example 12 565.7 475.6 15.7 Embodiment 13 571.6 481.5 16.0 Embodiment 14 577.3 487.2 16.4 Embodiment 15 581.6 494.1 16.6 Example 16 585.4 494.7 16.9 Comparative Example 1 517.4 410.9 13.5 Comparative Example 2 428.3 365.6 11.4

Claims

1. A lightweight high-pressure resistant aluminum alloy material, characterized in that: The composite material is composed of pretreated high-pressure resistant aerogel particles and an aluminum alloy substrate, wherein the addition amount of the pretreated high-pressure resistant aerogel particles is 5.0-13.0% of the aluminum alloy substrate; the aluminum alloy substrate is composed of the following components: Si is 0.2-1.0%; Mg: 0.5-1.5%; Zn: 0.2- 0.5%; Ce: 0.2-0.35% The balance is Al; The preparation method of the high pressure resistant aerogel particles is as follows: S11: Mixing the brucite fiber dispersion and the silica sol and stirring evenly, adding the konjac glucomannan aqueous solution and stirring evenly to obtain a wet gel; the mass fraction of the brucite fiber in the brucite fiber dispersion is 10-20%; the length of the brucite fiber is 0.1-2.0 μm; the content of konjac glucomannan in the konjac glucomannan aqueous solution is 15-22wt.%; the volume ratio of the brucite fiber dispersion, the silica sol and the konjac glucomannan aqueous solution is (5-10):100:(10-25); S12: freezing the wet gel to obtain a frozen block gel; S13: vacuum drying the block gel to obtain a porous composite gel; S14: sintering the porous composite gel at a high temperature of 700-800° C., and crushing the porous composite gel to obtain high pressure resistant aerogel particles; The particle size of the high pressure resistant aerogel particles is 0.05-0.1 μm; The pretreatment method of the pretreated high pressure resistant aerogel particles is: Step 1: Dissolve 13 parts of magnesium nitrate hexahydrate and 6 parts of sodium carbonate in 50 parts of water to obtain a magnesium nitrate solution and a sodium carbonate solution; Step 2: Place 40 parts of high pressure resistant aerogel particles in a magnesium nitrate solution, add a sodium carbonate solution, and stir and mix thoroughly; Step 3: Aging for 3 hours, filtering the precipitate, washing it thoroughly with distilled water, and then washing it with ethanol; Step 4: Place in an oven at 80°C for 4 hours and then calcine at 600°C for 3 hours.

2. The method for preparing a lightweight high-pressure resistant aluminum alloy material according to claim 1, characterized in that: The preparation steps are as follows: S1: Melt the aluminum alloy substrate, add the pretreated high-pressure resistant aerogel particles, and stir at a speed of 80-100 rpm for 20 minutes; S2: Increase the stirring speed and stir at 300-400 rpm for 10-20 min; S3: Cast into a mold and cool naturally in the air.