Preparation method of 3D structure fog collecting material with super hydrophilicity and super hydrophobicity

The superhydrophilic-superophobic 3D structural surface is prepared by electrochemical anodizing method and spraying method, which solves the problem of low fog collection efficiency in the prior art, and realizes efficient fog capture and rapid rolling down, with a wide range of Application prospects.

CN116288361BActive Publication Date: 2024-11-15HUBEI UNIV
0 Cites 0 Cited by

Patent Information

Application Number
CN202310341660.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-11-15
Estimated Expiration
2043-04-03

Smart Images

  • Figure CN116288361B_ABST
    Figure CN116288361B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a 3D structure fog collecting material with super hydrophilic-super hydrophobic properties. Inspired by the concave-convex-concave structure of corrugated paper, a three-dimensional structure material with hybrid wettability is prepared by electrochemical anodization, spraying, photocatalysis and template methods. This hybrid wettability of the concave-convex-concave matching surface can greatly improve the fog water collection efficiency during the fog water collection process. The fog flow interacts with the 3D structure to form a tubular vortex in the depression. This tubular vortex connected up and down helps the surface to quickly capture large droplets, and the surface water collection efficiency of the super hydrophilic-super hydrophobic hybrid wettability is also higher than that of a single wettability surface. Therefore, based on its excellent water collection ability, the three-dimensional structure material with hybrid wettability can be promoted on a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hybrid wettability surface preparation, and particularly relates to a method for preparing a surface material with high efficiency in fog water collection. Background Art

[0002] The uneven distribution of water resources around the world, climate change and increasingly serious water pollution problems have led to a shortage of fresh water resources worldwide. Collecting water resources in fog has also become a breakthrough in solving the hidden danger of water shortage in some arid areas. However, research and development of special structures or surfaces that can efficiently collect fresh water resources from fog remains a challenge. Hybrid wettability combined with three-dimensional structure can provide ideas for the preparation of efficient fog collection materials. First, the 3D structure has a larger surface area in direct contact with the fog flow than the 2D plane, and the 3D structure can effectively reduce the deviation of the fog flow. Second, the droplets on the hybrid wettability surface can be quickly captured and condensed into large droplets by the superhydrophilic sites on the surface, and then easily roll off from the superhydrophobic area of ​​the surface. This can effectively improve the efficiency of fog water collection of the material. The superhydrophilic-superhydrophobic 3D structure fog collection material prepared by the present invention is expected to have broad application prospects in the field of fog water collection.

[0003] The present invention prepares super-hydrophilic ZnO by electrochemical anodization. Combining the spraying method and the photocatalytic reaction, PDMS is grafted on ZnO to obtain a super-hydrophobic surface. A super-hydrophilic-super-hydrophobic 3D structure is prepared by the template method and the mask method. The fog collection efficiency of this hybrid wettability three-dimensional material is much higher than that of the original 2D plane, which is 418% of the original zinc sheet. At the same time, it is improved by 168% compared with the super-hydrophilic-super-hydrophobic hybrid 2D plane, and by 150% compared with the super-hydrophobic 3D structure. Based on the above excellent performance, the 3D structure fog collection material can be promoted on a large scale. Summary of the invention

[0004] The purpose of the present invention is to provide a large-scale and efficient method for preparing a super-hydrophilic-super-hydrophobic 3D structure fog collecting material. The super-hydrophilic ZnO and the hydrophobicity of PDMS are used to obtain hybrid wettability, and a zinc sheet with a corrugated paper structure is prepared by pressing using a template method. The preparation of a hybrid wettability 3D structure fog collecting material is achieved.

[0005] The technical solution to achieve the purpose of the present invention is: a method for preparing a super-hydrophilic-super-hydrophobic 3D structure fog collecting material, characterized in that it comprises the following steps:

[0006] A. Preparation of super-hydrophilic ZnO: A corrugated paper-like zinc sheet with a certain bending angle was prepared by template pressing, and the bending angle θ satisfied 30°≤θ≤120°. The zinc sheet was placed in acetone, anhydrous ethanol and deionized water for 10 min of ultrasonic treatment to remove surface dirt. The cleaned zinc sheet was then electropolished in a 7:3 ethanol / phosphoric acid solution at a constant voltage of 15 V for 3 min. Subsequently, the zinc sheet was electrochemically anodized for 45 min at a constant voltage of 8 V, and the obtained ZnO was annealed in air at 200°C for 120 min to improve its integrity and crystallinity.

[0007] B. Preparation of superhydrophobic PDMS@ZnO: First, the superhydrophilic ZnO was immersed in the PDMS solution for 20 min, and then the sample covered with a layer of PDMS was placed horizontally under a UV lamp for 30 min; finally, the excess ungrafted PDMS was washed away with tetrahydrofuran and dried under a nitrogen flow;

[0008] C. Preparation of superhydrophilic-superhydrophobic hybrid zinc sheet: First, dilute PDMS and cover the surface part that needs to remain superhydrophilic with a mask; then spray the diluted PDMS solution onto the superhydrophilic ZnO surface for 3 times at a spraying distance of 20 cm; then remove the mask and place the sample covered with a thin layer of PDMS horizontally under a UV lamp for 30 minutes; finally, use tetrahydrofuran to wash away the excess ungrafted PDMS and dry it under a nitrogen flow.

[0009] Preferably, in step A, the size of the imitation corrugated paper zinc sheet is 4 cm×6 cm.

[0010] Preferably, in step A, the bending angle of the imitation corrugated paper zinc sheet is 60°≤θ≤120°.

[0011] Furthermore, in step A, the best effect is achieved when the bending angle of the imitation corrugated paper zinc sheet is θ=60°.

[0012] Preferably, in step B, the mass percentage ratio of polydimethylsiloxane PDMS and curing agent is: 90.91%:9.09%.

[0013] Preferably, in step B and step C, the sample is placed under a 20 W ultraviolet lamp for 30 min at a distance of 10 cm.

[0014] Preferably, in step C, PDMS is diluted at a volume ratio of n-hexane to PDMS of 20:1.

[0015] Preferably, in step C, the purity of tetrahydrofuran is analytical, and the purity is ≥99.0%.

[0016] Compared with the prior art, the advantages of the present invention are:

[0017] 1. The preparation process is simple, the raw materials are easily available, and the cost is low.

[0018] 2. The surface sprayed with PDMS was used, and the prepared surface had good sliding properties.

[0019] 3. The surface of the PDMS is soaked and photocatalytically grafted under ultraviolet irradiation, which has good antifouling performance and self-cleaning ability.

[0020] 4. Due to the use of superhydrophilic-superhydrophobic hybrid surface and 3D structure, the final surface has excellent fog water collection efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The following is a flow chart of the preparation of the super-hydrophobic ZnO sheet of the present invention, and SEM images of different samples obtained during the preparation process. (ab) Super-hydrophilic ZnO sheet; (cd) Super-hydrophobic ZnO sheet sprayed with PDMS coating.

[0022] Figure 2 Preparation and morphology characterization diagram of the present invention. (ab) SEM and EDS spectra of super-hydrophilic ZnO surface; (cd) SEM and EDS spectra of super-hydrophobic ZnO surface prepared by immersion method; (ej) SEM, apparent contact angle and EDS spectra of super-hydrophobic ZnO surface prepared by spraying method, the number of spraying is 2, 3 and 4 times respectively, and the spraying distance is 20cm.

[0023] Figure 3 The antifouling and self-cleaning test diagrams of the present invention. (a) Antifouling performance test of superhydrophobic ZnO surface, the three liquids are cola, coffee, and milk; (b) Self-cleaning performance test of superhydrophobic ZnO surface; (c) Adhesion characterization of superhydrophobic ZnO surface; (d) Changes of surface contact angle and sliding angle with UV irradiation time after spraying PDMS coating; (e) The bouncing process of droplets on superhydrophobic ZnO surface.

[0024] Figure 4The effect of the 3D structure and hybrid wettability of the present invention on water collection efficiency. (a) Comparison of the weight of water collected by the original zinc sheet and the 3D structured zinc sheet within 0.5 h; (b) 2D plane water collection model; (c) 3D structure water collection model; (d) Bar graph of water collection efficiency of the original zinc sheet, superhydrophilic ZnO sheet, superhydrophobic ZnO sheet and superhydrophilic-superhydrophobic hybrid ZnO sheet. The hybrid surface has three superhydrophilic bands, 4 cm long, 2 mm wide, and 1 cm apart; (e) Relationship between the time and droplet diameter of the first drop of the original zinc sheet surface, superhydrophilic surface, superhydrophobic surface and superhydrophilic-superhydrophobic hybrid surface; (f) Optical photos of contact angles of the original zinc sheet surface, superhydrophilic surface, superhydrophobic surface and superhydrophilic-superhydrophobic hybrid surface. Droplets of different colors come from aqueous solutions dyed with different dyes.

[0025] Figure 5 The effect of depressions and tips on water collection efficiency in the 3D structure of the present invention. Both structural surfaces are super hydrophobic surfaces. (a) The aggregation process of droplets in the mist flow on the concave-convex-concave structure; (b) The aggregation process of droplets in the mist flow on the convex-concave-convex structure; (c) The bar graph of water collection efficiency of super hydrophobic surfaces with two different concave-convex structures; (d) Optical photos of droplet nucleation, growth, and rolling at the depression; (e) Optical photos of droplet nucleation, growth, and rolling at the convex tip.

[0026] Figure 6 Optical photos of the droplet nucleation, growth aggregation and shedding process at different angles of the super-hydrophobic 3D structure depression and the super-hydrophobic 2D plane of the present invention. (a) Super-hydrophobic 2D surface; (b) Super-hydrophobic 3D structure depression at θ=30°; (c) Super-hydrophobic 3D structure depression at θ=60°; (d) Super-hydrophobic 3D structure depression at θ=120°.

[0027] Figure 7 The comprehensive fog collection capacity diagram of the present invention. (a) is a bar graph of the water collection efficiency of the superhydrophobic 3D structure with different angles of the present invention, θ=30°; θ=60°; θ=120°; (b) a linear graph of the water collection weight of the superhydrophobic 3D structure with different angles within 2 h, collected once every half an hour; (c) a schematic diagram of the fog collection process, with a fog flow rate of 0.8 m / s; (d) a bar graph of the water collection efficiency of the fog collector combined with different hybrid wettabilities and 3D structures, respectively, superhydrophilic-superhydrophobic 3D structure, only three concave bottom straight lines are superhydrophilic, and θ=60°; superhydrophilic-superhydrophobic 3D structure, only two convex tip straight lines are superhydrophilic, and θ=60°; superhydrophilic-superhydrophobic 3D structure, three concave straight lines and two convex tip straight lines are superhydrophilic, and the rest are superhydrophobic, and θ=60°.

[0028] Figure 8The figure is a study on the behavior of droplets in the fog collection process of the present invention. (a) Bar graph of water collection efficiency within 2 hours for the original zinc sheet, superhydrophilic-superhydrophobic hybrid 2D plane, superhydrophobic 3D structure, and superhydrophilic tip-superhydrophobic 3D structure (one cycle every half hour); (b) Linear graph of water collection weight within 2 hours. One cycle every half hour; (c) Optical photograph of droplet nucleation, growth, aggregation and shedding process on superhydrophilic-superhydrophobic hybrid 2D surface; (d) Optical photograph of droplet nucleation, growth, aggregation and shedding process in superhydrophilic depression; (e) Optical photograph of droplet nucleation, growth, aggregation and shedding process at superhydrophilic tip. Implementation

[0029] The present invention will be described in more detail below through specific examples, but the protection scope of the present invention is not limited to these embodiments. Example

[0030] 1. Preparation of super-hydrophilic ZnO: Corrugated paper-like zinc sheets (4 cm×6 cm) with three bending angles (θ=30°, 60°, 120°) were prepared by template pressing. The zinc sheets were placed in acetone, anhydrous ethanol and deionized water for 10 min to remove surface dirt. The cleaned zinc sheets were then electropolished in a 7:3 ethanol / phosphoric acid solution at a constant voltage of 15 V for 3 min. Subsequently, a constant voltage of 8 V was selected, and the zinc sheet was electrochemically anodized for 45 min. The obtained ZnO was annealed in air at 200°C for 120 min to improve its integrity and crystallinity.

[0031] 2. Preparation of superhydrophobic PDMS@ZnO: First, the superhydrophilic ZnO was immersed in the PDMS solution for 20 min, and then the sample covered with a layer of PDMS was placed horizontally under a UV lamp (20 W) for 30 min at a distance of about 10 cm. Finally, the excess ungrafted PDMS was washed away with tetrahydrofuran and dried under a nitrogen flow.

[0032] 3. Preparation of super-hydrophilic-super-hydrophobic hybrid zinc sheet: First, dilute PDMS (diluted according to the volume ratio of n-hexane and PDMS at 20:1), and mask the part of the surface that needs to remain super-hydrophilic. Then spray the diluted PDMS solution onto the super-hydrophilic ZnO surface 3 times at a spraying distance of 20 cm. Then remove the mask, and place the sample covered with a thin layer of PDMS horizontally under a UV lamp for 30 minutes at a distance of about 10 cm. Finally, use tetrahydrofuran to wash away the excess ungrafted PDMS and dry it under a nitrogen stream.

[0033] 4. From the electron microscope morphology, it can be seen that the super-hydrophilic surface is composed of closely connected pore structures, and from the further enlarged SEM image, it can be seen that these closely connected pore structures are composed of long and thin ZnO nanowires. Figure 1 (ab). Then, the super-hydrophilic ZnO sheet that has undergone high temperature annealing is immersed in the PDMS solution for 20 minutes and then irradiated with ultraviolet light for 30 minutes to obtain a super-hydrophobic ZnO sheet with a surface morphology as shown in FIG. Figure 2 (c). The surface microstructure is similar to that of super-hydrophilic ZnO sheets, but the difference is that the surface contact angle is about 154.4°. Super-hydrophobic ZnO sheets can also be obtained by directly spraying PDMS solution on the super-hydrophilic surface and then UV curing. However, the short ZnO nanowires on the surface obtained by spraying are tightly connected into bundles. Figure 1 As shown in (cd), it can be seen that the originally long and thin ZnO nanowires are broken into short sections of ZnO nanowires, and these short ZnO nanowires are tightly connected. Example

[0034] 1. Preparation of super-hydrophilic ZnO: Corrugated paper-like zinc sheets (4 cm×6 cm) with three bending angles (θ=30°, 60°, 120°) were prepared by template pressing. The zinc sheets were placed in acetone, anhydrous ethanol and deionized water for 10 min to remove surface dirt. The cleaned zinc sheets were then electropolished in a 7:3 ethanol / phosphoric acid solution at a constant voltage of 15 V for 3 min. Subsequently, a constant voltage of 8 V was selected, and the zinc sheet was electrochemically anodized for 45 min. The obtained ZnO was annealed in air at 200°C for 120 min to improve its integrity and crystallinity.

[0035] 2. Preparation of superhydrophobic PDMS@ZnO: First, the superhydrophilic ZnO was immersed in the PDMS solution for 30 min, and then the sample covered with a layer of PDMS was placed horizontally under a UV lamp (20 W) for 30 min at a distance of about 10 cm. Finally, the excess ungrafted PDMS was washed away with tetrahydrofuran and dried under a nitrogen flow.

[0036] 3. Preparation of super-hydrophilic-super-hydrophobic hybrid zinc sheet: First, dilute PDMS (diluted according to the volume ratio of n-hexane and PDMS at 20:1), and mask the part of the surface that needs to remain super-hydrophilic. Then spray the diluted PDMS solution onto the super-hydrophilic ZnO surface 3 times at a spraying distance of 20 cm. Then remove the mask, and place the sample covered with a thin layer of PDMS horizontally under a UV lamp for 30 minutes at a distance of about 10 cm. Finally, use tetrahydrofuran to wash away the excess ungrafted PDMS and dry it under a nitrogen stream.

[0037] 4. The antifouling and self-cleaning performance tests were carried out on the super-hydrophobic surface prepared by the immersion method. As shown in Figure 3 (a), the samples were immersed in cola, coffee, and milk for 10 s respectively. After being taken out, it can be found that there is no obvious residue on the surface of the sample after soaking in cola and coffee, but only a slight residue on the surface after soaking in milk, and the surface is restored after being rinsed with deionized water. This is enough to prove that the sample has good antifouling performance. As for the self-cleaning ability of the surface, Figure 3 As shown in (b), after the surface is stained with black dirt, the sample is rinsed with deionized water and no black residue remains on the surface of the sample, proving that the sample has excellent self-cleaning ability. Example

[0038] 1. Preparation of super-hydrophilic ZnO: Corrugated paper-like zinc sheets (4 cm×6 cm) with three bending angles (θ=30°, 60°, 120°) were prepared by template pressing. The zinc sheets were placed in acetone, anhydrous ethanol and deionized water for 10 min to remove surface dirt. The cleaned zinc sheets were then electropolished in a 7:3 ethanol / phosphoric acid solution at a constant voltage of 15 V for 3 min. Subsequently, a constant voltage of 8 V was selected, and the zinc sheet was electrochemically anodized for 45 min. The obtained ZnO was annealed in air at 200°C for 120 min to improve its integrity and crystallinity.

[0039] 2. Preparation of superhydrophobic PDMS@ZnO: First, the superhydrophilic ZnO was immersed in the PDMS solution for 30 min, and then the sample covered with a layer of PDMS was placed horizontally under a UV lamp (20 W) for 30 min at a distance of about 10 cm. Finally, the excess ungrafted PDMS was washed away with tetrahydrofuran and dried under a nitrogen flow.

[0040] 3. Preparation of super-hydrophilic-super-hydrophobic hybrid zinc sheet: First, dilute PDMS (diluted according to the volume ratio of n-hexane and PDMS at 20:1), and mask the part of the surface that needs to remain super-hydrophilic. Then spray the diluted PDMS solution onto the super-hydrophilic ZnO surface, spraying 4 times at a spraying distance of 20 cm. Then remove the mask, and place the sample covered with a thin layer of PDMS horizontally under a UV lamp for 30 minutes at a distance of about 10 cm. Finally, use tetrahydrofuran to wash away the excess ungrafted PDMS and dry it under a nitrogen stream.

[0041] 4. Water collection performance test: The prepared super-slippery surface was placed in a homemade fog collection tester (the fog flow rate and rate were 0.5 gs -1 and 2.4 ms -1), the distance between the sample and the mist outlet was about 20 cm. The test temperature and relative humidity were 25 °C and 90%, respectively. The water collection efficiency was improved, and the SHL-SHB sample was prepared by combining the superhydrophilic surface's ability to quickly capture droplets with the superhydrophobic surface's ability to quickly remove droplets. In order to speed up the removal of droplets in the superhydrophilic area, the superhydrophilic area of ​​the SHL-SHB is stripe-shaped, 4 cm long and 2 mm wide, with a total of three hydrophilic stripes on the surface, and the spacing between adjacent stripes is 1 cm. The optical photograph of droplets on the superhydrophilic-superhydrophobic hybrid surface is shown in Figure 2. Figure 4 As shown in (f), the droplets spread in the superhydrophilic area and maintain a rounded shape in the superhydrophobic area. However, due to the limitation of the superhydrophobic area, some droplets did not completely spread in the superhydrophilic area, which is conducive to the aggregation of droplets. The droplet shedding time and shedding size on the SHL-SHB surface are shown in Figure 2. Figure 4 As shown in (e), the droplet shedding time of the superhydrophobic area and the superhydrophilic area is slightly longer than that of the single superhydrophobic surface and the superhydrophilic surface, but the droplet shedding size is basically the same as that of the single superhydrophobic surface and the superhydrophilic surface. Compared with the single wettability surface, the initial droplet capture, transportation and removal cycle time of the hybrid wettability surface is longer. However, with the increase of the number of cycles, the droplet capture, transportation and removal cycle of the SHL-SHB surface is significantly accelerated, and its average water collection efficiency after multiple water collection is the highest, reaching 0.83 g cm-2 h-1( Figure 4 (d)). Example

[0042] 1. Preparation of super-hydrophilic ZnO: Corrugated zinc sheets (4 cm×6 cm) with three bending angles (θ=0°, 30°, 60°, 120°) were prepared by template pressing. The zinc sheets were placed in acetone, anhydrous ethanol and deionized water for 10 minutes to remove surface dirt. The cleaned zinc sheets were then electropolished in a 7:3 ethanol / phosphoric acid solution at a constant voltage of 15 V for 3 minutes. Subsequently, a constant voltage of 8 V was selected, and the zinc sheet was electrochemically anodized for 45 minutes. The obtained ZnO was annealed in air at 200°C for 120 minutes to improve its integrity and crystallinity.

[0043] 2. Preparation of superhydrophobic PDMS@ZnO: First, the superhydrophilic ZnO was immersed in the PDMS solution for 30 min, and then the sample covered with a layer of PDMS was placed horizontally under a UV lamp (20 W) for 30 min at a distance of about 10 cm. Finally, the excess ungrafted PDMS was washed away with tetrahydrofuran and dried under a nitrogen flow.

[0044] 3. Preparation of super-hydrophilic-super-hydrophobic hybrid zinc sheet: First, dilute PDMS (diluted according to the volume ratio of n-hexane and PDMS at 20:1), and mask the part of the surface that needs to remain super-hydrophilic. Then spray the diluted PDMS solution onto the super-hydrophilic ZnO surface, spraying 4 times at a spraying distance of 20 cm. Then remove the mask, and place the sample covered with a thin layer of PDMS horizontally under a UV lamp for 30 minutes at a distance of about 10 cm. Finally, use tetrahydrofuran to wash away the excess ungrafted PDMS and dry it under a nitrogen stream.

[0045] 4. The effect of bending angle on water collection efficiency can be explored by observing a water collection cycle on these surfaces with different bending angles. Figure 6 The optical photos of droplet capture, droplet transport, and droplet removal in the depressions of SHB-2D and the super-hydrophobic 3D structure of imitation corrugated paper with different bending angles. The SHB-2D surface has strong water repellency, which causes the droplets to be spherical on the super-hydrophobic 2D plane and roll off easily. Figure 6 As shown in (a), droplets began to roll down 15 seconds after water collection, and the droplets were very small and remained in a round shape. Figure 6 Optical photos of different surfaces after 60 s of water collection in (ad) show that compared with the 2D plane that causes the mist flow to deviate, the tubular vortex formed by the collision between the 3D structure imitating corrugated paper and the mist flow can allow the surface to capture more and larger droplets. The tubular vortex generated by the interaction between the 3D structure and the mist flow at different bending angles is different in size. The narrower the depression, the smaller the tubular vortex, that is, the smaller the θ, the smaller the tubular vortex. Figure 6 As shown in (b), the large droplets on the surface with θ = 30° begin to fall after 50 s of water collection; Figure 6 In (c), the droplet on the surface with θ = 60° starts to roll off at 35 s; Figure 6 In (d), the droplet on the surface with θ = 120° begins to fall off at 40 s. This shows that among the three surfaces, the surface with θ = 60° takes the shortest time to complete a water collection cycle, followed by the surface with θ = 120°, and the surface with θ = 30° takes the lowest time.

[0046] Summary: The present invention is inspired by the concave-convex-concave structure of corrugated paper, and a three-dimensional structural material with hybrid wettability is prepared by electrochemical anodization, spraying, photocatalysis and template methods. This hybrid wettability of the concave-convex-concave matching surface can greatly improve the efficiency of fog water collection during the fog water collection process. The fog flow interacts with the 3D structure to form a tubular vortex in the depression. This tubular vortex connected up and down helps the surface to quickly capture large droplets, and the surface water collection efficiency of the superhydrophilic-superhydrophobic hybrid wettability is also higher than that of a single wettability surface. Therefore, based on its excellent water collection ability, the three-dimensional structural material with hybrid wettability can be promoted on a large scale.

[0047] Although the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention.

Claims

1. A method for preparing a 3D structure fog collecting material with super hydrophilicity and super hydrophobicity, characterized in that: The steps include: A. Preparation of super-hydrophilic ZnO: A corrugated paper-like zinc sheet with a certain bending angle was prepared by template pressing, and the bending angle θ satisfied θ=60°. The zinc sheet was placed in acetone, anhydrous ethanol and deionized water for 10 min of ultrasound to remove surface dirt; then the cleaned zinc sheet was electropolished in a 7:3 ethanol / phosphoric acid solution at a constant voltage of 15 V for 3 min; Subsequently, the ZnO sheets were electrochemically anodized for 45 min at a constant voltage of 8 V, and the obtained ZnO was annealed in air at 200 °C for 120 min to improve its integrity and crystallinity; B. Preparation of superhydrophilic-superhydrophobic hybrid zinc sheet: First, dilute PDMS and cover the surface part that needs to remain superhydrophilic with a mask; then spray the diluted PDMS solution onto the superhydrophilic ZnO surface for 3 times at a spraying distance of 20 cm; then remove the mask and place the sample covered with a thin layer of PDMS horizontally under a UV lamp for 30 minutes; finally, use tetrahydrofuran to wash away the excess ungrafted PDMS and dry it under a nitrogen flow.

2. The method for preparing a super-hydrophilic-super-hydrophobic 3D structure fog collecting material according to claim 1, characterized in that: In step A, the size of the imitation corrugated paper zinc sheet is 4 cm×6 cm.

3. The method for preparing a super-hydrophilic-super-hydrophobic 3D structure fog collecting material according to claim 1, characterized in that: In step B, place under a 20 W UV lamp for 30 min at a distance of 10 cm.

4. The method for preparing a 3D structured fog collecting material having super hydrophilicity and super hydrophobicity according to claim 1, characterized in that: In step B, PDMS was diluted at a volume ratio of n-hexane to PDMS of 20:

1.

5. The method for preparing a super-hydrophilic-super-hydrophobic 3D structure fog collecting material according to claim 1, characterized in that: In step B, the purity of tetrahydrofuran is analytical, and the purity is ≥99.0%.