A kind of high elasticity high temperature resistant spandex fiber and preparation method thereof
By using silica composite microspheres in spandex fibers, combined with 4-methacryloyloxytrimellitic anhydride and salicylanilide, the problems of poor hygroscopicity and insufficient high temperature resistance are solved, and high elasticity and high temperature resistance are achieved The hydrophilic and oil-repellent effect improves the overall performance of the fabric.
Patent Information
- Application Number
- CN202310308960.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-28
AI Technical Summary
The existing spandex fibers have poor hygroscopicity and insufficient high-temperature resistance, which leads to the fabric breaking, yellowing and loosening during high-temperature dyeing, which cannot meet the market's demand for high elasticity and high-temperature resistance.
Silica composite microspheres were prepared by sol-gel method, 4-methacryloyloxytrimellitic anhydride and salicylanilide were added, and silicon carbide staple fiber and aminosiloxane were combined to form a surface-enriched hydrophilic group. The group of silica composite microspheres are doped in polyurethane prepolymers to enhance the high temperature resistance and hydrophilic oil repellency of the fibers.
It significantly improves the high temperature resistance and hydrophilic oil repellency of spandex fibers, improves hygroscopicity, enhances the elasticity and comfort of the fibers, and ensures the stability and strength of the fabric under high temperature conditions.
Smart Images

Figure CN116288767B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional chemical fibers, and in particular relates to a high-elasticity and high-temperature-resistant spandex fiber and a preparation method thereof. Background Art
[0002] Chemical fiber refers to fibers made from natural or synthetic high polymers through chemical processing. Among them, spandex fiber occupies an important position in chemical fibers. Spandex fiber is the abbreviation of polyurethane fiber. It is a highly elastic fiber that can be stretched 6-7 times. It can quickly return to its original state with the disappearance of tension and has a high elastic recovery rate. In addition to excellent resilience, spandex fiber also has excellent resistance to chemical degradation, acid and alkali resistance, sweat resistance, seawater resistance, dry cleaning resistance, wear resistance and other properties. It is often blended with other yarns such as cotton, polyester, nylon, cuprammonium fiber, etc., and is widely used in the field of stretch fabric weaving.
[0003] Spandex fibers are mainly divided into two categories, one is polyester chain, which has strong anti-oxidation and oil resistance; the other is polyether chain, which has outstanding mildew resistance and washing resistance. However, spandex fibers also have many disadvantages, such as poor hygroscopicity, affecting wearing comfort, poor heat resistance, and cannot withstand high-temperature ironing. When interwoven and blended with polyester, high-temperature dyeing will cause the spandex part to break, turn yellow, and become loose, resulting in the elasticity of the fabric being damaged and the size and shape becoming larger. With the expansion of the application field of spandex and the improvement of people's living standards, higher requirements are put forward for the resilience, high temperature resistance and other properties of spandex. The existing spandex fibers can no longer meet the existing market demand due to the limitations of the formula and preparation method. Based on the above statement, there is an urgent need to develop a spandex fiber with high elasticity and high temperature resistance. Summary of the invention
[0004] The purpose of the present invention is to solve the defects in the prior art and provide a silica composite microsphere for preparing high-elasticity and high-temperature resistant spandex fiber. The obtained spandex fiber has good hydrophilicity and oil repellency and excellent mechanical properties.
[0005] The purpose of the present invention is achieved through the following technical solutions.
[0006] In a first aspect, the present invention provides a silica composite microsphere, wherein the silica composite microsphere comprises 4-methacryloyloxy trimellitic anhydride and salicylanilide in a mass ratio of 2.4-3:1.
[0007] The silicon dioxide composite microspheres specifically include the following components:
[0008] 45-55 parts by weight of silica gel, 18-30 parts by weight of silicon carbide staple fibers, 10-20 parts by weight of aminosiloxane, 3-7 parts by weight of 4-methacryloyloxy trimellitic anhydride, 1-2.5 parts by weight of salicylanilide, and 2-5 parts by weight of initiator.
[0009] Wherein, the weight ratio of 4-methacryloyloxy trimellitic anhydride to salicylanilide is 2.4-3:1.
[0010] The silica composite microspheres are prepared by using tetraethyl orthosilicate as a precursor, p-toluenesulfonic acid and citric acid as catalysts, and anhydrous ethanol as a solvent. The silica gel is obtained by a sol-gel method, and then mixed with 4-methacryloyloxy trimellitic anhydride, salicylanilide, silicon carbide staple fibers, and aminosiloxane, and then added into an oil phase to stir the gel, and then aged in anhydrous ethanol to obtain the silica gel.
[0011] The silica composite microspheres are specifically prepared by the following method:
[0012] 1) Mix ethyl orthosilicate, anhydrous ethanol and deionized water, add p-toluenesulfonic acid and citric acid as catalysts, heat to 40-50° C. for hydrolysis to obtain silica gel, then introduce nitrogen for 1-2 hours under stirring to remove oxygen, and set aside;
[0013] 2) Under nitrogen protection, 4-methacryloyloxy trimellitic anhydride and salicylanilide are added to the silica gel, an initiator is added, and after stirring for 2-6 hours, silicon carbide staple fibers and aminosiloxane are added while stirring, and microwave treatment is performed for 20-50 minutes to obtain a silica composite gel;
[0014] 3) Using vegetable oil as the oil phase, add the silica composite gel dropwise while stirring, the volume ratio of the oil phase to the silica sol is 2.5-6:1, continue stirring until gelling, then add anhydrous ethanol, stir thoroughly and let stand to separate, separate the solid and liquid, wash with water, soak in ethanol for aging, dry and crush to obtain silica composite microspheres.
[0015] It should be noted that in step 1), the mass ratio of ethyl orthosilicate, anhydrous ethanol, p-toluenesulfonic acid, citric acid, and deionized water is 100:20-30:1-3:2-5:15-20.
[0016] It should be noted that the diameter of the silicon carbide short fibers is 10-50 nm and the length is 80-200 nm.
[0017] Note that the aminosiloxane is any one of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 3-aminopropyl-triethoxysilane, 3-aminopropyl-methyldimethoxysilane, and 3-aminopropyl-methyldiethoxysilane.
[0018] The present invention provides the above-mentioned silica composite microspheres. First, silica gel is prepared by a sol-gel method, and then the silica gel is mixed with 4-methacryloyloxy trimellitic anhydride, salicylanilide, silicon carbide staple fibers, and aminosiloxane to prepare the silica composite microspheres. The silica composite microspheres have a particle size in the range of 300-800nm, a large number of hydrophilic groups such as hydroxyl groups and amino groups are enriched on the surface, the silica composite microspheres have high activity and good hydrophilicity, and can be uniformly dispersed in a polyurethane prepolymer to avoid a decrease in fiber strength, improve the defect of poor hygroscopicity of spandex fibers, improve moisture absorption and oil repellency, and increase comfort. The presence of 4-methacryloyloxy trimellitic anhydride and salicylanilide in the silica composite microspheres has a synergistic effect and can significantly improve the high temperature resistance of the fibers. This may be because the presence of 4-methacryloyloxy trimellitic anhydride and salicylanilide effectively increases the crystallinity of polyurethane, thereby greatly improving the high temperature resistance of the fibers.
[0019] In a second aspect, the silica composite microspheres described in the first aspect are used to prepare high-elasticity and high-temperature resistant spandex fibers.
[0020] The application includes improving the high temperature resistance of spandex fibers.
[0021] The application also includes improving the hydrophilic and oil-repellent properties of spandex fibers.
[0022] In a third aspect, the present invention further provides a method for preparing a high-elasticity, high-temperature-resistant spandex fiber, comprising:
[0023] 1) preparing a modified polyether glycol-based fiber-forming polymer, wherein the modified polyether glycol-based fiber-forming polymer is a 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide-modified polytetramethylene ether glycol fiber-forming polymer;
[0024] 2) mixing the modified polyether diol-based fiber-forming polymer, the silica composite microspheres described in the first aspect, and additives to prepare a mixed spinning solution;
[0025] 3) Prepare spandex fibers by dry spinning.
[0026] The additives include anti-ultraviolet agent, antioxidant, lubricant; wherein,
[0027] The anti-ultraviolet agent is any one of UV-320, UV-326 and UV-531;
[0028] The antioxidant is any one of antioxidant T502, antioxidant T245, and antioxidant 425;
[0029] The lubricant is magnesium stearate.
[0030] The present invention adopts the above technical scheme, firstly, utilizes polytetramethylene ether glycol to react with diisocyanate to obtain -NCO-terminated polyurethane prepolymer, then utilizes epoxy group in 3-methyl-3-(p-toluenesulfonyloxymethyl) propylene oxide to react with terminal -NCO group for modification, obtains modified polyether glycol-based fiber-forming polymer, then blends with hydrophilic silica composite microspheres and additives to obtain spinning solution with good stability, and finally spins spandex fiber through dry spinning. By controlling the ratio of each component and spinning conditions, the spandex fiber has stable size and good uniformity, and has the properties of hydrophilicity, oil repellency, high elasticity, high temperature resistance and high strength.
[0031] The modified polyether diol-based fiber-forming polymer is prepared by prepolymerizing polytetramethylene ether glycol, a chain extender and diphenylmethane diisocyanate to obtain an isocyanate-terminated polyurethane prepolymer, and then reacting with 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide under the action of a catalyst.
[0032] The modified polyether glycol-based fiber-forming polymer is specifically prepared by the following method:
[0033] 1) mixing the dehydrated polytetramethylene ether glycol, a chain extender and 4,4-diphenylmethane diisocyanate in a molar ratio of 1:0.6-1:1.4-2.5, adding butyl tin dilaurate and stirring to react to obtain a prepolymer;
[0034] 2) adding N,N-dimethylacetamide to the prepolymer obtained in step 1, stirring the reaction to obtain a polyurethane prepolymer containing -NCO at both ends;
[0035] 3) Add 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide and a catalyst to the polyurethane prepolymer obtained in step 2), raise the temperature to 140-160° C. for reaction, and stop the reaction when the -NCO content in the reaction system drops to 0.1% to obtain a modified polyether diol-based fiber-forming polymer.
[0036] It should be noted that the number average molecular weight of polytetramethylene ether glycol is 1500-3000.
[0037] It should be noted that the chain extender is a mixture of polycaprolactone triol and any one of trimethylolethane, propylene glycol and trimethylolpropane, and the mixing molar ratio is 1:0.3-0.5.
[0038] It should be noted that the molar ratio of 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide, catalyst, and polytetramethylene ether glycol is 0.2-0.3:0.01-0.05:1.
[0039] The invention firstly utilizes polytetramethylene ether glycol and diisocyanate to react to obtain -NCO-terminated polyurethane prepolymer, and then utilizes 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide to modify the prepolymer. Rigid groups are introduced into the modified fiber-forming polymer molecules, so that the strength and high temperature resistance of the material are improved, and the cross-linking degree of the polyurethane is reduced, thereby avoiding the defect of decreased material resilience due to excessive cross-linking, thereby improving the resilience of the spandex fiber.
[0040] The specific steps of preparing the mixed spinning solution are:
[0041] Add silica composite microspheres, anti-ultraviolet agent, antioxidant and lubricant to N,N-dimethylacetamide, mix ultrasonically for 30-70 minutes, then add modified polyether diol-based fiber-forming polymer, stir and mix for 2-5 hours, then heat to 40-55°C, stir and mature for 18-30 hours to obtain a spinning mixture, and the viscosity of the spinning solution is 250-400 Pa·s.
[0042] It should be noted that the contents of each component in the mixed spinning solution are: 0.5-2 parts by weight of anti-ultraviolet agent, 0.2-1 parts by weight of antioxidant, 0.1-1 parts by weight of lubricant, 20-28 parts by weight of modified polyether diol-based fiber-forming polymer, 3-8 parts by weight of silica composite microspheres, and 60-75 parts by weight of N,N-dimethylacetamide.
[0043] The specific parameters of the dry spinning are: the diameter of the spinneret holes is 0.10-0.20 mm, and the distance between the holes is 1.0-3.0 mm.
[0044] In a fourth aspect, a high-elasticity, high-temperature-resistant spandex fiber is prepared by the method described in the third aspect.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] 1) In the present invention, a polyether diol-based fiber-forming polymer modified with 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide is mixed with silica composite microspheres and additives to obtain a mixed spinning solution, and then the mixed spinning solution is dry-spun to obtain a spandex fiber. Compared with conventional spandex fibers, the spandex fiber has improved elastic recovery rate and high temperature resistance, and has the advantages of high strength, hydrophilicity and oil repellency.
[0047] 2) Silica composite microspheres are added to spandex fibers, wherein the presence of 4-methacryloyloxy trimellitic anhydride and salicylanilide has a synergistic effect, which can significantly improve the high temperature resistance of the fiber. The presence of hydrophilic groups makes it have high hygroscopicity and oil repellency, thereby improving the defect of poor hygroscopicity of spandex fibers, increasing comfort, and improving the oil repellency of the fibers;
[0048] 3) Modification of polyether diol-based fiber-forming polymers by 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide introduces rigid groups into the polyurethane molecules, thereby improving the strength and high temperature resistance of the material and increasing the resilience of the spandex fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 is an infrared spectrum of the spandex fiber of Example 1 of the present invention;
[0050] Figure 2 Schematic diagram of moisture regain test results of the spandex fiber of the present invention;
[0051] Figure 3 Schematic diagram of the oil contact angle test results of the spandex fiber of the present invention;
[0052] Figure 4 It is a schematic diagram of the tensile strength test results of the spandex fiber of the present invention;
[0053] Figure 5 It is a schematic diagram of the test result of 300% elastic recovery rate of the spandex fiber of the present invention;
[0054] Figure 6 It is a schematic diagram of the thermal deformation temperature test results of the spandex fiber of the present invention. DETAILED DESCRIPTION
[0055] The technical solution of the present invention is further described in detail below in conjunction with specific implementation modes and drawings.
[0056] Embodiment 1: A high elasticity and high temperature resistant spandex fiber:
[0057] The high-elasticity and high-temperature-resistant spandex fiber is prepared by the following method:
[0058] 1) Preparation of silica composite microspheres: 100 g of tetraethyl orthosilicate, 26 g of anhydrous ethanol, 2.5 g of p-toluenesulfonic acid, 4 g of citric acid, and 18.5 g of deionized water were mixed, heated to 40° C. for hydrolysis to obtain silica composite microspheres, and then nitrogen was introduced for 2 h under stirring at 200 r / min to remove oxygen for standby use; under nitrogen protection, 5.6 g of 4-methacryloyloxy trimellitic anhydride and 2 g of salicylanilide were added to 48.4 g of silica composite microspheres, i.e., the mass ratio of 4-methacryloyloxy trimellitic anhydride to salicylanilide was 2.8:1, 4 g of initiator potassium persulfate was added, and stirred at 300 r / min for 4 h Then, 24 g of silicon carbide staple fibers (with a diameter of 35 nm and a length of 140 nm) and 16 g of 3-aminopropyl-methyldimethoxysilane were added while stirring, and the mixture was subjected to microwave treatment for 30 min at a microwave power of 600 W to obtain a silica composite gel; soybean oil was used as the oil phase, and the silica composite gel was added dropwise under stirring at 200 r / min, with a volume ratio of the oil phase to the silica sol of 5:1. After the addition, stirring was continued until gelation occurred, and then ethanol was added, and the mixture was allowed to stand for stratification after sufficient stirring, and the mixture was separated from the solid and liquid, washed with water, and immersed in ethanol for aging, dried at 50°C, and crushed to obtain silica composite microspheres with an average particle size of 428 nm;
[0059] 2) Preparation of modified polyether diol-based fiber-forming polymer: 1 mol of polytetramethylene ether glycol (number average molecular weight of 2000) vacuum dehydrated at 140°C was mixed with 0.8 mol of chain extender and 2.2 mol of diphenylmethane diisocyanate in a molar ratio of 1:0.8:2.2, wherein the chain extender was polycaprolactone triol and trimethylolethane in a molar ratio of 1:0.4, and 0.02 mol of butyl tin dilaurate was added and stirred to obtain a prepolymer at a stirring rate of 200 r / min. min, then add N,N-dimethylacetamide in an amount of 2 times the weight of the prepolymer to the prepolymer, stir for 1 hour to obtain a polyurethane prepolymer containing isocyanate groups at both ends; then add 0.26 mol 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide and 0.03 mol 2-ethyl-4-methylimidazole to the polyurethane prepolymer, raise the temperature to 150° C. for reaction, and stop the reaction when the -NCO content in the reaction system drops to 0.1% to obtain a modified polyether diol-based fiber-forming polymer;
[0060] 3) Preparation of mixed spinning solution: 60 g of the hydrophilic silica composite microspheres obtained in step 1), 10 g of UV-326, 6 g of antioxidant T245, and 4 g of magnesium stearate were added to 660 g of N, N-dimethylacetamide at a frequency of 20 kW and a power density of 0.35 W / cm 2The mixture was ultrasonicated for 40 min under the conditions of , then 260 g of modified polyether diol-based fiber-forming polymer was added, stirred at 400 r / min for 4 h, and then heated to 50 ° C and stirred and aged for 24 h to obtain a spinning mixture with a viscosity of 300 Pa·s;
[0061] 4) Dry spinning: 40D spandex fiber was spun by dry spinning. During the spinning process, the diameter of the spinneret holes was 0.15 mm and the distance between the holes was 2.0 mm.
[0062] The spandex fiber obtained in this embodiment was tested by infrared spectrum using Nicolet 5700 infrared spectrometer, and the results were as follows: Figure 1 As shown in the figure, it can be seen that 2250cm -1 Nearby is the absorption peak of -NCO, 1642cm -1 、1548cm -1 Nearby is the absorption peak of carbamate, 1105cm -1 、802cm -1 Nearby is the absorption peak of Si-O-Si bond, 1220cm -1 Nearby is the coupling peak between Si-O-Si and COC, at 1190 cm -1 、1368cm -1 Nearby, an absorption peak attributed to the sulfonyloxy group in 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide appeared. The above results show that 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide successfully modified the polyurethane.
[0063] Embodiment 2: Another high elasticity and high temperature resistant spandex fiber:
[0064] The high-elasticity and high-temperature-resistant spandex fiber is prepared by the following method:
[0065] 1) Preparation of silica composite microspheres: The only difference from step 1) in Example 1 is that: under nitrogen protection, 4.8 g of 4-methacryloyloxy trimellitic anhydride and 2 g of salicylanilide are added to 50 g of silica composite microspheres, that is, the mass ratio of 4-methacryloyloxy trimellitic anhydride to salicylanilide is 2.4:1, 3.2 g of potassium persulfate is added, and after stirring for 3 hours, 24 g of silicon carbide staple fibers (diameter 40 nm, length 140 nm) and 16 g of 3-aminopropyl-methyldimethoxysilane are added while stirring, and stirring is continued for 2 hours to obtain a silica composite gel; the remaining raw materials, reaction steps and experimental conditions are the same as step 1) in Example 1;
[0066] 2) Preparation of modified polyether diol-based fiber-forming polymer: the raw materials, reaction steps and experimental conditions are the same as those in step 2) of Example 1;
[0067] 3) preparing a mixed spinning solution: the raw materials, reaction steps and experimental conditions are the same as those in step 3) of Example 1;
[0068] 4) Dry spinning: the raw materials, reaction steps and experimental conditions are the same as those in step 4) of Example 1;
[0069] Embodiment 3: Another high elasticity and high temperature resistant spandex fiber:
[0070] The high-elasticity and high-temperature-resistant spandex fiber is prepared by the following method:
[0071] 1) Preparation of silica composite microspheres: The only difference from step 1) in Example 1 is that: under nitrogen protection, 6 g of 4-methacryloyloxy trimellitic anhydride and 2 g of salicylanilide are added to 47 g of silica composite microspheres, that is, the mass ratio of 4-methacryloyloxy trimellitic anhydride to salicylanilide is 3:1, 5 g of potassium persulfate is added, and after stirring for 4 hours, 24 g of silicon carbide staple fibers (diameter 40 nm, length 140 nm) and 16 g of 3-aminopropyl-methyldimethoxysilane are added while stirring, and stirring is continued for 3 hours to obtain a silica composite gel; the remaining raw materials, reaction steps and experimental conditions are the same as step 1) in Example 1;
[0072] 2) Preparation of modified polyether diol-based fiber-forming polymer: the raw materials, reaction steps and experimental conditions are the same as those in step 2) of Example 1;
[0073] 3) preparing a mixed spinning solution: the raw materials, reaction steps and experimental conditions are the same as those in step 3) of Example 1;
[0074] 4) Spandex fibers were prepared by dry spinning; the raw materials, reaction steps and experimental conditions were the same as those in step 4) of Example 1.
[0075] Comparative Example 1: Another high-elasticity, high-temperature-resistant spandex fiber:
[0076] The preparation method of spandex fiber in this comparative example is different from that in Example 1 only in that: in the process of preparing silica composite microspheres, an equal amount of salicylanilide is used instead of 4-methacryloyloxytrimellitic anhydride and salicylanilide, that is, 4-methacryloyloxytrimellitic anhydride is not added; the remaining raw materials, reaction steps and experimental conditions are the same as those in Example 1.
[0077] Comparative Example 2: Another high-elasticity, high-temperature-resistant spandex fiber:
[0078] The preparation method of the spandex fiber in this comparative example is different from that in Example 1 only in that: in the process of preparing the silica composite microspheres, an equal amount of 4-methacryloxy trimellitic anhydride is used instead of 4-methacryloxy trimellitic anhydride and salicylanilide, that is, salicylanilide is not added; the remaining raw materials, reaction steps and experimental conditions are the same as those in Example 1.
[0079] Comparative Example 3: Another high-elasticity, high-temperature-resistant spandex fiber:
[0080] The preparation method of spandex fiber in this comparative example is different from that in Example 1 only in that 4-methacryloyloxy trimellitic anhydride and salicylanilide are not added during the preparation of silica composite microspheres; the remaining raw materials, reaction steps and experimental conditions are the same as those in Example 1.
[0081] Comparative Example 4: Another high-elasticity, high-temperature-resistant spandex fiber:
[0082] The preparation method of spandex fiber in this comparative example is different from that in Example 1 only in that no silica composite microspheres are added; the remaining raw materials, reaction steps and experimental conditions are the same as those in Example 1.
[0083] Comparative Example 5: Another high-elasticity, high-temperature-resistant spandex fiber:
[0084] The preparation method of spandex fiber in this comparative example differs from that in Example 1 only in that: in the step of preparing the modified polyether diol-based fiber-forming polymer, 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide is not used for modification; the remaining raw materials, reaction steps and experimental conditions are the same as those in Example 1.
[0085] The spandex fibers prepared in Examples 1-3 and Comparative Examples 1-5 were respectively subjected to the following tests to verify the beneficial effects of the technical solution of the present invention.
[0086] Experimental Example 1: Moisture regain test:
[0087] The moisture regain of spandex fiber was tested by using the mass difference before and after full drying. Each sample was tested 10 times and the average value was taken. The moisture regain R was calculated as follows:
[0088]
[0089] In formula (1),
[0090] M0—the weight of spandex fiber before fully drying;
[0091] M1—The mass of spandex fiber after being fully dried.
[0092] The moisture regain results are as follows: Figure 2 shown.
[0093] from Figure 2 Data observation shows that the moisture regain of the spandex fibers obtained in Examples 1-3 is not less than 2.5%, and the moisture regain of the spandex fibers obtained in Comparative Example 4 is lower than that in Examples 1-3, which indicates that the addition of silica composite microspheres to the spandex fibers helps to improve the defect of poor hygroscopicity of the spandex fibers, and the moisture regain is improved. The moisture regain of Comparative Example 1-2 is lower than that of Examples 1-3, but higher than that of Comparative Example 3, which indicates that the addition of a certain mass ratio of 4-methacryloyloxy trimellitic anhydride and salicylanilide to the silica composite microspheres is more conducive to improving the hygroscopicity of the spandex fibers; the moisture regain data of the spandex fibers obtained in Comparative Example 5 show that the modification of the polyether diol-based fiber-forming polymer has no obvious effect on the hygroscopicity of the fibers; comprehensive Figure 1 It can be seen from the data that the hygroscopicity of the spandex fiber prepared by the scheme of the present invention is improved, the comfort is increased, and the defects of the existing spandex fiber are compensated.
[0094] Experimental Example 2: Oil repellency:
[0095] The spandex fibers were spun into fabrics, and the oil contact angle of the fabrics was tested using a KrussDSA30 contact angle analyzer. Hexadecane was used as the test oil sample, and each sample was tested 20 times.
[0096] The oil contact angle was measured as Figure 3 shown.
[0097] from Figure 3 From the data observation, it is known that the oil contact angle of the spandex fiber obtained in Examples 1-3 is higher than 125°, indicating that it has a good oil repellent effect; compared with Examples 1-3, the oil contact angle of the spandex fiber obtained in Comparative Example 4 is greatly reduced, indicating that the addition of silica composite microspheres helps to improve the oil repellency of the spandex fiber; the oil contact angle of the spandex fiber obtained in Comparative Example 1-3 is lower than that in Examples 1-3, indicating that the addition of a certain proportion of 4-methacryloyloxytrimellitic anhydride and salicylanilide to the silica composite microspheres is more conducive to improving the oil repellency of the spandex fiber; and the oil contact angle of the spandex fiber obtained in Comparative Example 5 is not significantly decreased compared with that in Examples 1-3, indicating that the modification of the polyether diol-based fiber-forming polymer has little effect on the oil repellency of the fiber.
[0098] Experimental Example 3: Tensile Strength:
[0099] With reference to standard FZ / T50006-2013, the tensile strength at break was measured using a 5965 universal material testing machine produced by Instron, USA, and each sample was tested 20 times.
[0100] The tensile strength results are as follows Figure 4 shown.
[0101] from Figure 4From the data observation, it is known that the tensile strength of the spandex fiber obtained in Examples 1-3 is relatively high. Compared with Examples 1-3, the strength of the spandex fiber obtained in Comparative Example 1-3 is greatly reduced, while the strength of the spandex fiber in Comparative Example 4 is not significantly reduced, indicating that adding a certain mass ratio of 4-methacryloyloxytrimellitic anhydride and salicylanilide to the silica composite microspheres helps to make it evenly dispersed in the polyurethane and avoid reducing the strength of the fiber; compared with Examples 1-3, the strength of the spandex fiber obtained in Comparative Example 5 is greatly reduced, indicating that the modification of the polyether diol-based fiber-forming polymer has a good gain effect on the strength of the fiber.
[0102] Experimental Example 4: Rebound performance:
[0103] With reference to standard FZ / T50007-2012, the 300% elastic recovery rate of the fiber was tested using a 5965 universal material testing machine produced by Instron Corporation of the United States, and each sample was tested 20 times.
[0104] The results of the 300% elastic recovery rate are as follows: Figure 5 shown.
[0105] from Figure 5 From the data observation, it is known that the spandex fibers obtained in Examples 1-3 have high elastic recovery rate and good resilience; compared with Examples 1-3, the elastic recovery rate of the spandex fibers obtained in Comparative Example 1-4 has no obvious decrease, which indicates that the addition of silica composite microspheres has no obvious effect on the resilience of the fibers; while the elastic recovery rate of the spandex fibers obtained in Comparative Example 5 is greatly decreased, indicating that the modification of the polyether diol-based fiber-forming polymer has a good gain effect on the resilience of the fibers; the comprehensive tensile strength and elastic recovery rate results indicate that the spandex fibers obtained by the scheme described in the present invention can simultaneously have higher strength while ensuring higher resilience.
[0106] Experimental Example 5: High temperature resistance:
[0107] The heat deformation temperature of spandex fiber is tested according to the reference standard GB / T1634.1-2019.
[0108] The heat deformation temperature is measured as follows Figure 6 shown.
[0109] from Figure 6From the data observation, it is known that the heat deformation temperature of the spandex fiber obtained in Example 1 reaches 223.5°C, and the heat denaturation temperature of the preferred embodiments 1-3 is not less than 220°C, and the high temperature resistance is excellent; compared with embodiments 1-3, the heat deformation temperature of the spandex fibers obtained in comparative examples 1-4 decreased to varying degrees, which indicates that the addition of silica composite microspheres and the addition of 4-methacryloyloxytrimellitic anhydride and salicylanilide therein can significantly improve the high temperature resistance of the spandex fiber; the heat deformation temperature of the spandex fiber obtained in comparative example 5 is lower than that of embodiments 1-3, indicating that the modification of the polyether diol-based fiber-forming polymer has a good gain effect on the high temperature resistance of the fiber.
[0110] The conventional operations in the operating steps of the present invention are well known to those skilled in the art and will not be described in detail here.
[0111] The above embodiments are only used to illustrate the present invention, but not to limit the present invention. A person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions also belong to the scope of the present invention, and the patent protection scope of the present invention shall be defined by the claims.
Claims
1. A method for preparing high-elasticity and high-temperature resistant spandex fiber, characterized in that: include: 1) preparing a modified polyether glycol-based fiber-forming polymer, wherein the modified polyether glycol-based fiber-forming polymer is a 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide-modified polytetramethylene ether glycol fiber-forming polymer; 2) mixing the modified polyether diol-based fiber-forming polymer, silica composite microspheres, and additives to prepare a mixed spinning solution; 3) Preparation of spandex fibers by dry spinning; The silica composite microspheres contain 4-methacryloyloxy trimellitic anhydride and salicylanilide in a mass ratio of 2.4-3:1; The silica composite microspheres are prepared by using tetraethyl orthosilicate as a precursor, p-toluenesulfonic acid and citric acid as catalysts, and anhydrous ethanol as a solvent. The silica gel is obtained by a sol-gel method, and then mixed with 4-methacryloyloxy trimellitic anhydride, salicylanilide, silicon carbide staple fibers, and aminosiloxane, and then added into an oil phase to stir the gel, and then aged in anhydrous ethanol to obtain the silica gel.
2. The method according to claim 1, characterized in that The modified polyether diol-based fiber-forming polymer is prepared by prepolymerizing polytetramethylene ether glycol, a chain extender and diphenylmethane diisocyanate to obtain an isocyanate-terminated polyurethane prepolymer, and then reacting with 3-methyl-3-(p-toluenesulfonyloxymethyl)propylene oxide under the action of a catalyst.
3. The method according to claim 2, characterized in that The chain extender is a mixture of polycaprolactone triol and any one of trimethylolethane, propylene glycol and trimethylolpropane, and the mixing molar ratio is 1:0.3-0.
5.
4. The method according to claim 1, characterized in that: The specific steps of preparing the mixed spinning solution are: Add silica composite microspheres, anti-ultraviolet agent, antioxidant and lubricant to N,N-dimethylacetamide, mix ultrasonically for 30-70 minutes, then add modified polyether diol-based fiber-forming polymer, stir and mix for 2-5 hours, then heat to 40-55°C, stir and mature for 18-30 hours to obtain a spinning mixture, and the viscosity of the spinning solution is 250-400 Pa·s.
5. The method according to claim 1, characterized in that The specific parameters of dry spinning are: the diameter of the spinneret holes is 0.10-0.20 mm, and the distance between the holes is 1.0-3.0 mm.
6. High elasticity and high temperature resistant spandex fiber obtained by the method according to any one of claims 1 to 5.
Citation Information
Patent Citations
Method for preparing PP fiber-enhanced silica gel material
CN104446333A
Oral care composition containing silica and zinc citrate
CN106456461A
Method for preparing moisture absorption and sweat releasing polyurethane elastic fibers having skin core structure
CN108977929A
Puncture-resistant liquid-retaining organic-inorganic membrane for lithium battery and preparation method
CN111490214A
Rigid polyurethane foam produced from polyisocyanate and poly:ol mixt. - prepd. by reacting organic poly:isocyanate and poly:ol mixt. in presence of blowing agent and catalyst
DE2825498A1