Adhesive tape for semiconductor device manufacturing

By using adhesive tapes with substrate, ablation layer, barrier layer and first adhesive layer in semiconductor device manufacturing, laser ablation technology is used to achieve efficient peeling of chip components, and the peeling defects in the prior art are solved and The problem of residue adhesion improves yield and transfer efficiency.

CN116323194BActive Publication Date: 2024-12-03SEKISUI CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280006985.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-09-06
Filing Date
2022-09-05
Publication Date
2024-12-03
Estimated Expiration
2042-09-05

AI Technical Summary

Technical Problem

In the manufacturing of existing semiconductor devices, poor peeling of chip components and problem of adhesion of adhesive layer residues, resulting in low yield and difficulty in efficient transfer.

Method used

Adhesive tapes with a base material, ablation layer, a barrier layer and a first adhesive layer are used to deform the ablation layer by laser ablation, and pass the deformation to the barrier layer and adhesive layer, thereby improving the peeling performance of chip components. , and prevent the adhesive layer from cracking and residue adhesion.

Benefits of technology

The peeling performance of chip components is improved, the cracking of the adhesive layer and residue adhesion is reduced, the yield is enhanced, and the efficient transfer process is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004182002310000141
    Figure BDA0004182002310000141
  • Figure BDA0004182002310000161
    Figure BDA0004182002310000161
  • Figure BDA0004182002310000181
    Figure BDA0004182002310000181
Patent Text Reader

Abstract

The present invention aims to provide an adhesive tape for semiconductor device manufacturing which has excellent chip component peeling performance and can suppress residual adhesive on chip components. The present invention is an adhesive tape for semiconductor device manufacturing which has a substrate, an ablation layer, a barrier layer and a first adhesive layer in this order.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive tape for manufacturing a semiconductor device. Background Art

[0002] In the manufacturing process of a semiconductor device, a plurality of chip components arranged on an adhesive layer may be transferred onto a driving circuit substrate.

[0003] For example, a micro LED display is a display device in which the chips constituting each pixel are tiny light emitting diode (LED) chips, and the micro LED chips emit light by themselves to display images. Micro LED displays have high contrast and fast response speed. In addition, since they do not require color filters used in liquid crystal displays, organic EL displays, etc., they can also be made thinner, so they have attracted much attention as the next generation of display devices. In a micro LED display, multiple micro LED chips are densely laid out in a flat surface.

[0004] In the manufacturing process of semiconductor devices such as such a micro LED display, for example, a transfer laminate having a plurality of chip components arranged on an adhesive layer is placed opposite to a driving circuit substrate, and the chip components are peeled off from the transfer laminate and electrically connected to the driving circuit substrate (transfer process).

[0005] As the method for peeling off chip components from the transfer laminate, for example, it is known that the back side of the support of the transfer laminate is focused on the adhesive layer and the method of irradiating laser (for example, patent documentation 1). Such method is also referred to as laser ablation. In addition, the following method is also known: in the adhesive layer, heat-expandable particles, heat-expandable microcapsules, etc. are matched, and the heat-expandable particles, heat-expandable microcapsules, etc. are thermally expanded by the heat-compression bonding of the transfer laminate and the drive circuit substrate, thus, the chip components are peeled off (for example, patent documentation 2, 3) by reducing the bonding area caused by the deformation of the adhesive layer.

[0006] Prior Art Literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2019-138949

[0009] Patent Document 2: Japanese Patent Application Publication No. 2019-15899

[0010] Patent Document 3: Japanese Patent Application Publication No. 2003-7986 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, in the conventional method of peeling off the chip components, there is a problem that it is difficult to transfer the chip components with a high yield due to poor peeling of the chip components.

[0013] In addition, when laser ablation is performed using a conventional adhesive layer, there is also the problem of adhesive layer residues adhering to chip components. That is, although it is possible to peel off chip components by laser ablation by increasing the output power of the laser, sometimes the adhesive layer breaks when the chip components are peeled off, and the adhesive layer residues adhere to the chip components.

[0014] An object of the present invention is to provide an adhesive tape for semiconductor device manufacturing which has excellent chip component peeling performance and can suppress adhesive residue on chip components.

[0015] Means for solving problems

[0016] The present disclosure 1 is an adhesive tape for manufacturing a semiconductor device, which has a substrate, an ablation layer, a barrier layer, and a first adhesive layer in this order.

[0017] Present Disclosure 2 is the adhesive tape for semiconductor device manufacturing according to Present Disclosure 1, wherein the substrate is a resin film.

[0018] Present disclosure 3 is the adhesive tape for manufacturing a semiconductor device according to present disclosure 2, wherein the resin film is a polyester film.

[0019] Present disclosure 4 is an adhesive tape for semiconductor device manufacturing according to present disclosure 1, 2 or 3, wherein the ablative layer has an ultraviolet absorption rate of 90% or more at a wavelength of 365 nm.

[0020] The present disclosure 5 is an adhesive tape for manufacturing a semiconductor device according to the present disclosure 1, 2, 3 or 4, wherein the storage modulus G' of the ablation layer at 23°C is 1×10 4 Pa or more and 2×10 5 Below Pa.

[0021] Present disclosure 6 is the adhesive tape for manufacturing a semiconductor device according to present disclosure 1, 2, 3, 4 or 5, wherein the thickness of the barrier layer is 25 μm or less.

[0022] Present disclosure 7 is the adhesive tape for manufacturing a semiconductor device according to present disclosure 6, wherein the thickness of the barrier layer is 6 μm or less.

[0023] Present disclosure 8 is the adhesive tape for manufacturing a semiconductor device according to present disclosure 1, 2, 3, 4, 5, 6 or 7, wherein the barrier layer is a polyester film.

[0024] Present disclosure 9 is the pressure-sensitive adhesive tape for semiconductor device manufacturing according to present disclosure 1, 2, 3, 4, 5, 6, 7 or 8, wherein the barrier layer has an easily adhesive resin layer on a surface in contact with the first pressure-sensitive adhesive layer.

[0025] Present disclosure 10 is the adhesive tape for semiconductor device manufacturing according to present disclosure 1, 2, 3, 4, 5, 6, 7, 8 or 9, wherein the first adhesive layer has a breaking strength of 1 MPa or more.

[0026] Disclosure 11 is an adhesive tape for semiconductor device manufacturing according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, wherein the storage modulus G' of the first adhesive layer at 23°C is 1×10 4 Pa or more and 2×10 5 Below Pa.

[0027] Present disclosure 12 is the adhesive tape for semiconductor device manufacturing according to Present Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or 11, wherein the first adhesive layer contains an ABA type block copolymer.

[0028] Present disclosure 13 is the adhesive tape for semiconductor device manufacturing according to present disclosure 12, wherein in the ABA type block copolymer, block A contains a structure derived from an aromatic vinyl monomer, and block B contains a structure derived from a (meth)acrylic monomer.

[0029] Present disclosure 14 is the pressure-sensitive adhesive tape for semiconductor device manufacturing according to present disclosure 12 or 13, wherein the block B has a structure derived from a monomer having a crosslinkable functional group.

[0030] Present disclosure 15 is an adhesive tape for manufacturing a semiconductor device according to present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13 or 14, wherein the gel fraction of the first adhesive layer is 70 wt % or more and 95 wt % or less.

[0031] Disclosure 16 is an adhesive tape for semiconductor device manufacturing according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15, wherein the thickness of the first adhesive layer is 5 μm or more and 30 μm or less.

[0032] Disclosure 17 is an adhesive tape for manufacturing a semiconductor device according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or 16, wherein the rolling ball initial adhesion of the adhesive tape for manufacturing a semiconductor device is No. 5 or above.

[0033] Disclosure 18 is an adhesive tape for manufacturing a semiconductor device according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16 or 17, wherein the surface release strength of the first adhesive layer of the adhesive tape for manufacturing a semiconductor device is 1 MPa or less.

[0034] Disclosure 19 is an adhesive tape for manufacturing a semiconductor device according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 or 18, wherein the adhesion between the substrate and the ablation layer is 6 N / 25 mm or more.

[0035] Disclosure 20 is an adhesive tape for manufacturing a semiconductor device according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18 or 19, wherein the adhesion between the ablation layer and the barrier layer is 6 N / 25 mm or more.

[0036] The present disclosure 21 is an adhesive tape for manufacturing a semiconductor device according to the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, wherein the first adhesive layer is a curable adhesive layer.

[0037] Disclosure 22 is an adhesive tape for manufacturing a semiconductor device according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or 21, wherein it also has a second adhesive layer, so that the adhesive tape for manufacturing a semiconductor device has the second adhesive layer, the above-mentioned substrate, the above-mentioned ablation layer, the above-mentioned barrier layer and the above-mentioned first adhesive layer in sequence.

[0038] Disclosure 23 is an adhesive tape for manufacturing a semiconductor device according to Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21 or 22, wherein the adhesive tape for manufacturing a semiconductor device is used for manufacturing a semiconductor device having a laser irradiation process.

[0039] Hereinafter, the present invention will be described in detail.

[0040] The inventors of the present invention have discovered that an adhesive tape for manufacturing semiconductor devices having a substrate, an ablation layer, a barrier layer and a first adhesive layer in sequence can improve the peeling performance of chip components and suppress residual adhesive on chip components even when chip components are peeled off by laser ablation, thereby completing the present invention.

[0041] The adhesive tape for manufacturing a semiconductor device of the present invention comprises a substrate, an ablation layer, a barrier layer, and a first adhesive layer in this order.

[0042] By using the adhesive tape for manufacturing semiconductor devices of the present invention, by irradiating the ablation layer with laser, the portion of the ablation layer irradiated with laser can be deformed by ablation. In addition, since the deformation of the portion of the ablation layer irradiated with laser is transmitted to the barrier layer and the first adhesive layer, the chip component arranged on the first adhesive layer can be peeled off. In addition, at this time, the scattering of the ablation layer caused by ablation is suppressed by the barrier layer. Therefore, according to the adhesive tape for manufacturing semiconductor devices of the present invention, the peeling performance of the chip component can be improved, and the first adhesive layer can be prevented from being broken when the chip component is peeled off, and the residue of the first adhesive layer can be prevented from being attached to the chip component.

[0043] exist Figure 1 : A cross-sectional view schematically showing an example of a process of peeling off a chip component arranged on an adhesive layer by laser ablation using a conventional adhesive tape. Figure 1 In the process shown, a chip component 1 is arranged on an adhesive layer 4 laminated on a substrate 5, and the chip component 1 is peeled off by laser 8a irradiated from a laser irradiation device 8, and the chip component 1 is electrically connected to a drive circuit substrate 7 (transfer process). The laminate 9 of the substrate 5 and the adhesive layer 4 may be, for example, a conventional single-sided adhesive tape in which the substrate 5 is a substrate such as a resin film and the adhesive layer 4 is composed only of an adhesive layer; or a laminate of a support such as a glass substrate and an adhesive layer 4 is a conventional double-sided adhesive tape (which may have a substrate) and a double-sided adhesive tape.

[0044] exist Figure 1 In the process shown, if the adhesive layer 4 is irradiated with laser 8a, the portion of the adhesive layer 4 irradiated with laser 8a is deformed due to ablation. More specifically, if the adhesive layer 4 is irradiated with laser 8a, the molecules of the adhesive layer 4 are broken by heat and reduced in molecular weight, and evaporate instantly, or sublimate (decompose and evaporate) due to high temperature, so that the portion of the adhesive layer 4 irradiated with laser 8a is deformed. As a result, the chip component 1 can be peeled off. By using laser 8a, it is possible to cause the chip component 1 to be peeled off in an extremely small range, so that even in the case of an array of extremely small chip components such as micro LED chips, the chip component 1 can be peeled off individually and with high peeling performance. However, in Figure 1 In the process shown, as described above, there are problems that the chip component 1 may not be properly peeled off, or the adhesive layer 4 may be broken when the chip component 1 is peeled off, so that the residue of the adhesive layer 4 may adhere to the chip component 1 .

[0045] exist Figure 2: A cross-sectional view schematically showing an example of an adhesive tape for manufacturing a semiconductor device according to the present invention. Figure 2 In the adhesive tape 12 for manufacturing a semiconductor device of the present invention shown, a substrate 5, an ablation layer 10, a barrier layer 11, and a first adhesive layer 4a are laminated in this order.

[0046] exist Figure 3 : A cross-sectional view schematically showing an example of a process of peeling off a chip component arranged on an adhesive layer by laser ablation using the adhesive tape for manufacturing a semiconductor device of the present invention. Figure 3 In the process shown, it is also related to Figure 1 In the process shown in the figure, the chip component 1 is arranged on the first adhesive layer 4a, and the chip component 1 is peeled off by the laser 8a irradiated from the laser irradiation device 8. Figure 3 In the process shown, by irradiating the ablation layer 10 with the laser 8a, the portion of the ablation layer 10 irradiated with the laser 8a can be deformed by ablation. In addition, the deformation of the portion of the ablation layer 10 irradiated with the laser 8a is transmitted to the barrier layer 11 and the first adhesive layer 4a, so that the chip component 1 arranged on the first adhesive layer 4a can be peeled off. In addition, at this time, the scattering of the ablation layer 10 caused by ablation is suppressed by the barrier layer 11.

[0047] By having the above-mentioned substrate, the adhesive tape for manufacturing a semiconductor device of the present invention has appropriate stiffness and is excellent in handling properties.

[0048] The substrate is not particularly limited, but preferably has a moderate UV transmittance from the viewpoint of peeling the chip components by laser ablation. The UV transmittance of the substrate is not particularly limited, but the preferred lower limit of the UV transmittance at a wavelength of 365 nm is 1%, the more preferred lower limit is 50%, and the further preferred lower limit is 80%. The upper limit of the UV transmittance at a wavelength of 365 nm is not particularly limited, but substantially about 95% is the upper limit.

[0049] The ultraviolet transmittance of the substrate at a wavelength of 365 nm can be measured, for example, using a spectrophotometer (UV-2600i, manufactured by Shimadzu Corporation, or an equivalent thereof) in accordance with JIS L1925.

[0050] From the viewpoint of adjusting the ultraviolet transmittance at the wavelength of 365 nm to the above range, the substrate is preferably a resin film.

[0051] The resin film is not particularly limited, and is preferably a polyester film from the perspective of excellent heat resistance. As the polyester film, for example, films comprising polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, etc. can be cited. Among them, polyethylene terephthalate film is preferred. In addition, from the viewpoint of excellent ultraviolet transmittance, the resin film is preferably an acrylic resin film. As the acrylic resin film, for example, films comprising polymethyl methacrylate can be cited. In addition, as the resin film, for example, films comprising polyacetal, polyamide, polycarbonate, polyphenylene ether, ultra-high molecular weight polyethylene, syndiotactic polystyrene, polyarylate, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyimide, polyetherimide, fluororesin, liquid crystal polymer, etc. can also be cited.

[0052] The thickness of the substrate is not particularly limited, but the preferred lower limit is 5 μm and the preferred upper limit is 188 μm. By making the thickness of the substrate within the above range, an adhesive tape having moderate stiffness and excellent handling properties can be prepared. The more preferred lower limit of the thickness of the substrate is 12 μm, and the more preferred upper limit is 100 μm.

[0053] The haze of the substrate is not particularly limited, and from the viewpoint of making the laser transmit efficiently and further improving the peeling performance of the chip component, the haze is preferably small. The preferred upper limit of the haze of the substrate is 10%, the more preferred upper limit is 5%, and the further preferred upper limit is 1%. The lower limit of the haze of the substrate is not particularly limited, and the smaller the more preferred, the lower limit is substantially about 0.1%.

[0054] The haze of the substrate can be measured, for example, using a haze meter (NDH4000, manufactured by Nippon Denshoku Industries).

[0055] The ablation layer is not particularly limited as long as it is a layer that is deformed by ablation when irradiated with laser light, and may or may not have adhesive properties.

[0056] From the viewpoint of causing deformation caused by ablation by irradiating laser, the above-mentioned ablation layer preferably has a moderate ultraviolet absorption rate. The ultraviolet absorption rate of the above-mentioned ablation layer at a wavelength of 365nm is not particularly limited, and the preferred lower limit is 90%, and the more preferred lower limit is 99%. If the ultraviolet absorption rate at the above-mentioned wavelength of 365nm is within the above-mentioned range, the stimulation of the laser in the above-mentioned ablation layer is efficiently converted into heat or vibration, so that deformation caused by ablation is easily caused, and the peeling performance of the chip component of the adhesive tape for manufacturing semiconductor devices is further improved. The upper limit of the ultraviolet absorption rate at the above-mentioned wavelength of 365nm is not particularly limited, and substantially about 99.9% is the upper limit.

[0057] The ultraviolet absorption rate of the ablation layer at a wavelength of 365 nm can be measured, for example, using a spectrophotometer (UV-2600i, manufactured by Shimadzu Corporation, or an equivalent thereof) in accordance with JIS L1925.

[0058] From the viewpoint of adjusting the ultraviolet absorption rate at the wavelength of 365 nm to the above range, the ablation layer preferably contains an ultraviolet absorber.

[0059] The ultraviolet absorber is not particularly limited, and examples thereof include benzotriazole ultraviolet absorbers and hydroxyphenyl triazine ultraviolet absorbers. In addition, examples thereof include ethylhexyl methoxycinnamate, octyl methoxycinnamate, ethylhexyl p-methoxycinnamate, diethylaminohydroxybenzoyl hexyl benzoate, bis-ethylhexyloxyphenol methoxyphenyl triazine, tert-butyl methoxydibenzoylmethane, and the like. Among them, benzotriazole ultraviolet absorbers and hydroxyphenyl triazine ultraviolet absorbers are preferred from the viewpoint of excellent compatibility with other components in the ablation layer. These ultraviolet absorbers may be used alone or in combination of two or more.

[0060] The content of the ultraviolet absorber is not particularly limited, but the preferred lower limit is 4 parts by weight relative to 100 parts by weight of the base polymer contained in the ablation layer. If the content of the ultraviolet absorber is 4 parts by weight or more, the peeling performance of the chip component of the adhesive tape for manufacturing a semiconductor device is further improved. The more preferred lower limit of the content of the ultraviolet absorber is 6 parts by weight, the further preferred lower limit is 8 parts by weight, the further preferred lower limit is 10 parts by weight, and the further preferred lower limit is 15 parts by weight.

[0061] The upper limit of the content of the ultraviolet absorber is not particularly limited, but from the viewpoint of ensuring the adhesion between the ablative layer and the substrate or the barrier layer, the upper limit is preferably 30 parts by weight. It should be noted that if the adhesion between the ablative layer and the substrate or the barrier layer is insufficient, for example, when the adhesive tape for semiconductor device manufacturing is cut into a desired tape width, undesirable conditions such as floating (end floating) may sometimes occur at the cut end.

[0062] The storage modulus (shear storage modulus) G' of the ablation layer at 23°C and 1 Hz is not particularly limited, but the preferred lower limit is 1×10 4 Pa, the upper limit of which is preferably 2×10 5 Pa. If the storage modulus G' is within the above range, the ablation layer can be appropriately deformed by ablation by laser irradiation, and the peeling performance of the chip component of the adhesive tape for semiconductor device manufacturing is further improved. The more preferred lower limit of the storage modulus G' is 1.5×10 4Pa, and the more preferred upper limit is 1.5×10 5 Pa, and a further preferred lower limit is 2.0×10 4 Pa, and a further preferred upper limit is 1.0×10 5 Pa.

[0063] It should be noted that the storage modulus G' of the above-mentioned ablation layer at 23°C and 1 Hz can be obtained, for example, as the storage modulus at 23°C when a dynamic viscoelastic spectrum of -40 to 140°C is measured under the conditions of a heating rate of 5°C / min and 1 Hz in a simple heating mode using a viscoelastic spectrometer (manufactured by IT Measurement and Control Co., Ltd., DVA-200 or its equivalent).

[0064] The ablation layer may or may not have adhesiveness, but from the viewpoint of ensuring the adhesiveness between the ablation layer and the substrate, for example, suppressing the undesirable situation such as the end floating, the adhesiveness between the substrate and the ablation layer is preferably 6N / 25mm or more, more preferably 10N / 25mm or more. The upper limit of the adhesiveness between the substrate and the ablation layer is not particularly limited, and the preferred upper limit is 50N / 25mm.

[0065] In addition, from the viewpoint of ensuring the adhesion between the ablation layer and the barrier layer, for example, suppressing the undesirable situation such as the end floating, the adhesive force between the ablation layer and the barrier layer is preferably 6N / 25mm or more, more preferably 10N / 25mm or more. The upper limit of the adhesive force between the ablation layer and the barrier layer is not particularly limited, and the preferred upper limit is 50N / 25mm.

[0066] It should be noted that the adhesive force mentioned here can be obtained, for example, as follows: using Autograph (manufactured by Shimadzu Corporation) or the like, in accordance with JIS Z0237, a peel test is performed in an environment of temperature 23°C and relative humidity 50% at a tensile speed of 300 mm / min in a 180° direction, and the 180° adhesive force (N / 25 mm) is measured to obtain the adhesive force.

[0067] As the base polymer contained in the above-mentioned ablation layer, for example, ABA type block copolymers, acrylic copolymers, urethane copolymers, silicone adhesives, etc. can be cited. Among them, ABA type block copolymers and acrylic copolymers are preferred from the perspective of easily adjusting the storage modulus G' of the above-mentioned ablation layer to the above-mentioned range and further improving the peeling performance of the chip components of the adhesive tape for semiconductor device manufacturing. From the perspective of not becoming too large when the ablation layer is irradiated with laser, ABA type block copolymers are more preferred. In addition, from the perspective of ensuring the adhesion of the above-mentioned ablation layer to the above-mentioned substrate or the above-mentioned barrier layer, for example, suppressing the above-mentioned end floating and other undesirable conditions, acrylic copolymers are more preferred.

[0068] The ABA block copolymer and the acrylic copolymer as the base polymer contained in the ablation layer may be the same polymers as the ABA block copolymer and the acrylic copolymer as the base polymer contained in the first adhesive layer, which will be described later.

[0069] In the case where the base polymer contained in the ablation layer is an ABA type block copolymer, the SP value of the copolymer of the B block is not particularly limited, and is preferably 9.5 or more. By making the above-mentioned SP value above 9.5, the adhesion with the above-mentioned substrate and the above-mentioned barrier layer becomes good, and it is not easy to produce the peeling of the above-mentioned ablation layer when ablation occurs, which can further improve the peeling performance of the chip component. The above-mentioned SP value is more preferably above 9.6, and more preferably above 9.8. The upper limit of the above-mentioned SP value is not particularly limited, but due to the difficulty of synthesis, it is substantially about 14 as the upper limit.

[0070] It should be noted that the SP value is called a solubility parameter, which is a parameter used as an index of polarity. In this specification, the calculation of the SP value uses the Fedors method (RF Fedors, Polym. Eng. Sci., 14 (2), 147-154 (1974)). In addition, the SP value of the copolymer of the B block of the ABA type block copolymer can be calculated based on the SP value of each repeating unit in the copolymer of the B block, using its mixing ratio (molar ratio).

[0071] The thickness of the ablation layer is not particularly limited, but the preferred lower limit is 3 μm and the preferred upper limit is 50 μm. If the thickness of the ablation layer is within the above range, the ablation layer can be appropriately deformed by ablation by irradiating the laser, and the peeling performance of the chip component of the adhesive tape for manufacturing semiconductor devices is further improved. The more preferred lower limit of the thickness of the ablation layer is 5 μm, the more preferred upper limit is 30 μm, the further preferred lower limit is 8 μm, and the further preferred upper limit is 20 μm.

[0072] The gel fraction of the ablation layer is not particularly limited, but the preferred lower limit is 70% by weight, and the preferred upper limit is 95% by weight. If the gel fraction is 70% by weight or more, the peeling performance of the chip component of the adhesive tape for manufacturing semiconductor devices is further improved. If the gel fraction is 95% by weight or less, the holding performance of the chip component of the adhesive tape for manufacturing semiconductor devices is further improved. The more preferred lower limit of the gel fraction is 80% by weight, and the more preferred upper limit is 90% by weight.

[0073] It should be noted that the gel fraction of the ablation layer can be measured by the following method.

[0074] Only 0.1 g of the above-mentioned ablation layer (ablation layer composition) was taken out from the adhesive tape for manufacturing semiconductor devices, immersed in 50 mL of ethyl acetate, and shaken for 24 hours using a shaker at a temperature of 23°C and 200 rpm. After shaking, the ethyl acetate and the ablation layer composition that has swollen due to absorption of ethyl acetate were separated using a metal mesh (mesh #200 mesh). The separated ablation layer composition was dried at 110°C for 1 hour. The weight of the ablation layer composition including the metal mesh after drying was measured, and the gel fraction of the above-mentioned ablation layer was calculated using the following formula.

[0075] Gel fraction (wt%) = 100 × (W 1 -W 2 ) / W 0

[0076] (W 0 : Initial ablative layer composition weight, W 1 : Weight of the ablative layer composition containing the metal mesh after drying, W 2 : Initial weight of the metal mesh)

[0077] When the ablative layer composition cannot be completely dissolved in ethyl acetate, toluene, hexane, water or other solvents are used instead of ethyl acetate. Specifically, when the ablative layer composition contains a styrene elastomer, toluene or hexane is used, and when the ablative layer composition contains polyvinyl alcohol, hot water at 90° C. is used.

[0078] The barrier layer is not particularly limited as long as it can suppress the scattering of the ablation layer and can be deformed according to the deformation of the portion of the ablation layer irradiated with the laser. From the viewpoint of suppressing the scattering of the ablation layer and being deformed according to the deformation of the portion of the ablation layer irradiated with the laser, the barrier layer is preferably a resin film.

[0079] The resin film is not particularly limited, but from the viewpoint of suppressing the scattering of the ablation layer and being able to deform according to the deformation of the portion of the ablation layer irradiated with the laser, a polyester film and a polyolefin film are preferred, and a polyester film is more preferred. Examples of the polyester film include films made of polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and the like. Examples of the polyolefin film include films made of polyethylene, unstretched polypropylene, biaxially stretched polypropylene, cycloolefin polymers, cycloolefin copolymers, and the like.

[0080] In addition, examples of the resin film include films containing acrylic resins, polyacetals, polyamides, polycarbonates, polyphenylene ethers, syndiotactic polystyrene, polyarylates, polysulfones, polyethersulfones, polyphenylene sulfides, polyetheretherketones, polyimides, polyetherimides, fluororesins, liquid crystal polymers, and the like.

[0081] The barrier layer preferably has an easy-adhesion treatment layer on the surface of the side in contact with the first adhesive layer. By having the easy-adhesion treatment layer, the adhesion between the barrier layer and the first adhesive layer is further improved. The easy-adhesion treatment layer is not particularly limited, and examples thereof include a corona treatment layer, a primer treatment layer, and the like.

[0082] The thickness of the barrier layer is not particularly limited, but the preferred lower limit is 1 μm and the preferred upper limit is 25 μm. If the thickness of the barrier layer is 1 μm or more, the scattering of the ablation layer can be sufficiently suppressed. If the thickness of the barrier layer is 25 μm or less, the ablation layer can be sufficiently deformed according to the deformation of the laser-irradiated portion, and the peeling performance of the chip component of the adhesive tape for semiconductor device manufacturing is further improved. The more preferred lower limit of the thickness is 2 μm, the more preferred upper limit is 10 μm, and the more preferred upper limit is 6 μm.

[0083] The haze of the barrier layer is not particularly limited, but a smaller haze is preferred from the viewpoint of improving visibility and facilitating laser irradiation to an accurate portion of the chip, thereby further improving the peeling performance of the chip component. The upper limit of the haze of the barrier layer is preferably 10%, the upper limit is more preferably 5%, and the upper limit is further preferably 1%. The lower limit of the haze is not particularly limited, and the smaller the haze, the more preferred, but the actual lower limit is about 0.1%.

[0084] The haze of the barrier layer can be measured, for example, using a haze meter (NDH4000, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0085] The barrier layer may have an easy-adhesion resin layer on the surface in contact with the first adhesive layer. If the barrier layer has the easy-adhesion resin layer, the adhesion between the barrier layer and the first adhesive layer becomes higher, and the first adhesive layer is not easily peeled off from the barrier layer when transferring the chip, which can suppress the generation of residual adhesive on the chip.

[0086] The resin forming the easily adhesive resin layer is not particularly limited, and examples thereof include polyester resins, polyurethane resins, and nitrile rubber.

[0087] The highly adhesive resin layer may further contain known additives such as a plasticizer, a resin, a surfactant, a wax, a particulate filler, etc. These additives may be used alone or in combination of two or more.

[0088] The elastic modulus (MPa) of the above-mentioned easy-to-bond resin layer based on the nanoindentation method is not particularly limited, and the preferred lower limit is 4000MPa, and the preferred upper limit is 10000MPa. It should be noted that the elastic modulus of the above-mentioned resin layer based on the nanoindentation method can be obtained, for example, by the following method: using a nanoindenter (Hysitron Inc., Triboindenter TI-950), using a single indentation method at a specified temperature (25°C), under the measurement conditions of an indentation speed of 400nm / sec, a pull-out speed of 400nm / sec, and an indentation depth of 100nm, a diamond-made Berkovich-type (triangular pyramid-type) probe is vertically pressed on the measurement object layer, and the displacement-load hysteresis loop thus obtained is numerically processed by the software (triboscan) attached to the measurement device, thereby obtaining.

[0089] The thickness of the above-mentioned easy-adhesion resin layer is not particularly limited, and the preferred lower limit is 0.05μm, and the preferred upper limit is 0.3μm. If the thickness of the above-mentioned easy-adhesion resin layer is 0.05μm or more, the adhesion with the above-mentioned first adhesive layer becomes higher. If the thickness of the above-mentioned adhesive resin layer is 0.3μm or less, it is easy to deform during ablation, and the peeling performance of the chip component is further improved. The more preferred lower limit of the thickness of the above-mentioned easy-adhesion resin layer is 0.08μm, the more preferred upper limit is 0.2μm, the further preferred lower limit is 0.1μm, and the further preferred upper limit is 0.18μm.

[0090] The first adhesive layer is not particularly limited, but is preferably a pressure-sensitive adhesive layer. In addition, from the viewpoint of further improving the peeling performance of the chip component, the first adhesive layer may be a curable adhesive layer such as a thermosetting type or a photocurable type.

[0091] As the base polymer contained in the above-mentioned first adhesive layer, for example, ABA type block copolymer, acrylic copolymer, urethane copolymer, silicone adhesive etc. can be cited. Among them, from the aspect that the breaking strength, storage modulus G', gel fraction etc. of the above-mentioned first adhesive layer are easily adjusted to the range described later, the peeling performance of the chip component of the semiconductor device manufacturing adhesive tape is further improved, and the residual glue to the chip component can be further suppressed, preferably ABA type block copolymer and acrylic copolymer. From the same viewpoint, more preferably ABA type block copolymer.

[0092] The ABA type block copolymer is a copolymer including a block A (hereinafter also referred to as a “hard segment”) having a rigid structure and a block B (hereinafter also referred to as a “soft segment”) having a soft structure.

[0093] Regarding the above-mentioned ABA type block copolymer, the two blocks are difficult to be compatible, and sometimes the following structure is formed: the spherical islands formed by the aggregation of block A are scattered in the sea of ​​block B, and the cylindrical structure formed by the aggregation of the above-mentioned block A is scattered in the sea of ​​block B. The uneven phase separation structure. The phase separation structure in which such spherical islands are scattered is also referred to as a spherical (Japanese: スフィア-shaped) phase separation structure, and the phase separation structure in which the cylindrical structure is scattered is also referred to as a columnar (Japanese: シリンダー-shaped) phase separation structure. Moreover, by making the islands of the above-mentioned phase separation structure into pseudo crosslinking points, it is possible to give rubber elasticity to the above-mentioned ABA type block copolymer, so that it is easy to adjust the fracture strength, storage modulus G', gel fraction, etc. of the above-mentioned first adhesive layer to the range described later, and the peeling performance of the chip component of the adhesive tape for semiconductor device manufacturing is further improved, and the residual glue to the chip component can be further suppressed.

[0094] The ABA type block copolymer is preferably an ABA type triblock copolymer.

[0095] In the ABA type block copolymer, the block A is not particularly limited as long as it has a rigid structure, but preferably contains a structure derived from an aromatic vinyl monomer.

[0096] The block A may have, in addition to the structure derived from the aromatic vinyl monomer, a structure derived from a compound having a cyclic structure or a compound having a short side chain substituent, for example, within a range not impairing the effects of the present invention.

[0097] As the above-mentioned aromatic vinyl monomer, for example, styrene, α-methylstyrene, p-methylstyrene, chlorostyrene, etc. can be cited. These aromatic vinyl monomers can be used alone or in combination of two or more. Among them, styrene is preferred from the perspective of further improving the peeling performance of the chip components of the adhesive tape for semiconductor device manufacturing and further suppressing the residual glue on the chip components. It should be noted that in this specification, the structure derived from the aromatic vinyl monomer refers to a structure such as shown in the following general formula (1) or (2).

[0098] [Chemical formula 1]

[0099]

[0100] In the general formulas (1) and (2), R 1 represents a substituent having an aromatic ring. As a substituent R having an aromatic ring 1 , phenyl, methylphenyl, chlorophenyl and the like can be mentioned.

[0101] In the above-mentioned ABA type block copolymer, the content of the above-mentioned structure derived from the aromatic vinyl monomer is not particularly limited, and is preferably more than 1 weight % and less than 30 weight %. By making the content of the above-mentioned structure derived from the aromatic vinyl monomer the above-mentioned range, the fracture strength of the above-mentioned first adhesive layer becomes high, and the residual glue to the chip component can be further suppressed. The more preferred lower limit of the content of the above-mentioned structure derived from the aromatic vinyl monomer is 5 weight %, the further preferred lower limit is 8 weight %, the particularly preferred lower limit is 10 weight %, the more preferred upper limit is 28 weight %, the further preferred upper limit is 25 weight %, and the particularly preferred upper limit is 20 weight %.

[0102] In the above-mentioned ABA type block copolymer, the block B is not particularly limited as long as it has a soft structure. From the aspect of easily adjusting the breaking strength, storage modulus G', gel fraction, etc. of the above-mentioned first adhesive layer to the range described below, it is preferred to contain: a structure derived from a conjugated diene monomer or a structure derived from a (meth) acrylic acid monomer. From the aspect that the above-mentioned first adhesive layer can have more appropriate viscosity and the chip component holding performance of the adhesive tape for semiconductor device manufacturing is further improved, the block B more preferably contains a structure derived from a (meth) acrylic acid monomer.

[0103] The block B may have a structure derived from a monomer other than the conjugated diene monomer and the (meth)acrylic monomer, within a range not impairing the effects of the present invention.

[0104] As the above-mentioned conjugated diene monomer, for example, 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-octadiene, 1,3-hexadiene, 1,3-cyclohexadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, myrcene, chloroprene, etc. can be cited. These conjugated diene monomers can be used alone or in combination of two or more. Among them, 1,3-butadiene and isoprene are preferred from the aspect of high polymerization reactivity and easy industrial availability.

[0105] In the structure derived from the conjugated diene monomer, the double bond (unsaturated bond) can be converted into a saturated bond by hydrogenation. It should be noted that, for example, if the double bond (unsaturated bond) of the structure derived from 1,3-butadiene, which is the structure derived from the conjugated diene monomer, is hydrogenated, it is converted into an ethylene-butene structure. The ratio (hydrogenation rate) of the above hydrogenation is not particularly limited, and it can be partially hydrogenated or mostly hydrogenated.

[0106] It should be noted that the hydrogenation ratio (hydrogenation rate) can be measured by using deuterated chloroform as a solvent at 20 Hz. 1 It was calculated from the H-NMR spectrum.

[0107] In the above-mentioned ABA type block copolymer, the content of the structure derived from the above-mentioned conjugated diene monomer is not particularly limited, as long as the effect of the present invention is exerted, and is preferably 0% by weight or more and 99% by weight or less. The content of the structure derived from the above-mentioned conjugated diene monomer is more preferably 30% by weight or more, further preferably 40% by weight or more, further preferably 70% by weight or more, and further preferably 80% by weight or more. In addition, the content of the structure derived from the above-mentioned conjugated diene monomer is more preferably 95% by weight or less, and further preferably 90% by weight or less.

[0108] The content of the structure derived from the conjugated diene monomer is more preferably 70% by weight or more and 95% by weight or less, and further preferably 80% by weight or more and 90% by weight or less.

[0109] The (meth)acrylic acid monomer may be a single monomer or a plurality of monomers may be used. In the present specification, the structure derived from the (meth)acrylic acid monomer refers to a structure represented by the following general formula (5) or (6).

[0110] [Chemical formula 2]

[0111]

[0112] In the general formulas (5) and (6), R 3 Represents a side chain. As a side chain R 3, methyl, ethyl, propyl, butyl, isobutyl, pentyl, hexyl, cyclohexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, nonyl, isononyl, decyl, lauryl, stearyl, isostearyl, isobornyl and the like can be mentioned.

[0113] As the above-mentioned (meth) acrylic acid series monomer, for example, can be cited: methyl (meth) acrylate, ethyl (meth) acrylate, propyl (meth) acrylate, butyl (meth) acrylate, isobutyl (meth) acrylate, amyl (meth) acrylate, hexyl (meth) acrylate, cyclohexyl (meth) acrylate, heptyl (meth) acrylate, octyl (meth) acrylate, isooctyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, nonyl (meth) acrylate, isononyl (meth) acrylate, decyl (meth) acrylate, lauryl (meth) acrylate, stearyl (meth) acrylate, isostearyl (meth) acrylate, isobornyl (meth) acrylate, etc. These (meth) acrylic acid series monomers can be used alone or in combination of two or more. Among them, from the viewpoint of balancing the stripping performance of the chip component and the residual adhesive suppression effect to the chip component, butyl (meth) acrylate, 2-ethylhexyl (meth) acrylate and lauryl (meth) acrylate are preferred. From the viewpoint of further suppressing the residual adhesive on the chip components, butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are more preferred. In addition, their acrylates are more preferred.

[0114] In the above-mentioned ABA type block copolymer, the glass transition temperature of the above-mentioned block B is not particularly limited, and is preferably above -30°C and below 0°C. By making the glass transition temperature of the above-mentioned block B within the above-mentioned range, the peeling performance of the chip component of the adhesive tape is further improved even when transferring a chip component with a protrusion or a small-sized chip component, and the residual adhesive to the chip component can be further suppressed. The more preferred lower limit of the glass transition temperature of the above-mentioned block B is -28°C, the more preferred lower limit is -25°C, the more preferred upper limit is -5°C, and the more preferred upper limit is -10°C.

[0115] It should be noted that the glass transition temperature of the block B can be determined, for example, by using a differential scanning calorimeter (manufactured by TA Instruments, Hitachi High-Tech Science, etc.). More specifically, the following values ​​can be used: when the ABA type block copolymer is measured using a differential scanning calorimeter (manufactured by Hitachi High-Tech Science, SIIExstar 6000 / DSC 6220) under a nitrogen atmosphere and a heating rate of 10°C / min, the value obtained in the second round. It should be noted that the peak from the block A and the peak from the block B are obtained, and the peak on the low temperature side is taken as the peak from the block B, and the glass transition temperature of the block B is determined.

[0116] The method for adjusting the glass transition temperature of the block B to the above range is not particularly limited. In order to adjust the glass transition temperature of the block B to the above range, the (meth)acrylic monomer preferably contains a (meth)acrylate monomer having a glass transition temperature of 0° C. or higher when forming a homopolymer.

[0117] By making the (meth)acrylic acid-based monomer contain the (meth)acrylate monomer having a glass transition temperature of 0°C or more when forming a homopolymer, the storage modulus of the first adhesive layer can be adjusted to a more preferred range. Examples of the (meth)acrylate monomer having a glass transition temperature of 0°C or more when forming a homopolymer include: methyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, isobornyl acrylate, isobornyl methacrylate, and benzyl methacrylate. Methyl acrylate and methyl methacrylate are particularly preferred.

[0118] In the above-mentioned ABA type block copolymer, the content of the structure derived from the (meth) acrylate monomer having a glass transition temperature of 0°C or more when the homopolymer is prepared is not particularly limited, and can be 0% by weight, and the preferred lower limit is 35% by weight. If the content of the structure derived from the (meth) acrylate monomer having a glass transition temperature of 0°C or more when the homopolymer is prepared is 35% by weight or more, the peeling performance of the chip component of the adhesive tape is further improved. The more preferred lower limit of the content of the structure derived from the (meth) acrylate monomer having a glass transition temperature of 0°C or more when the homopolymer is prepared is 40% by weight.

[0119] The upper limit of the content of the structure derived from the (meth)acrylate monomer having a glass transition temperature of 0° C. or higher when forming a homopolymer is not particularly limited, but is preferably 60% by weight, and more preferably 50% by weight, from the viewpoint of temporarily fixing chip components.

[0120] The block B preferably further includes a structure derived from a monomer having a crosslinkable functional group.

[0121] By making the block B contain the structure derived from the monomer containing crosslinkable functional groups, the cohesive force of the first adhesive layer is improved due to the crosslinking of the crosslinkable functional groups, so that the peeling performance of the chip components of the adhesive tape for manufacturing semiconductor devices is improved, and the residual glue on the chip components can be suppressed. The crosslinkable functional groups can be crosslinked or not, and crosslinking is more preferred. However, even if the uncrosslinked structure is maintained, the cohesive force of the first adhesive layer can be improved by the interaction between the functional groups, the peeling performance of the chip components of the adhesive tape for manufacturing semiconductor devices is improved, and the residual glue on the chip components can be suppressed. It should be noted that in this specification, the structure derived from the monomer having a crosslinkable functional group refers to a structure such as that shown in the following general formula (3) or (4).

[0122] [Chemical formula 3]

[0123]

[0124] In the general formulas (3) and (4), R 2 represents a substituent containing at least one crosslinkable functional group. Examples of the crosslinkable functional group include a carboxyl group, a hydroxyl group, an epoxy group, a double bond, a triple bond, an amino group, an amide group, and a nitrile group. 2 An alkyl group, an ether group, a carbonyl group, an ester group, a carbonate group, an amide group, a carbamate group or the like may be contained as its constituent elements.

[0125] The above-mentioned monomer with crosslinking functional group is not particularly limited, for example, carboxyl-containing monomers, hydroxyl-containing monomers, epoxy-containing monomers, double-bond-containing monomers, triple-bond-containing monomers, amino-containing monomers, amide-containing monomers, nitrile-containing monomers, etc. can be cited. These monomers with crosslinking functional groups can be used alone or in combination of two or more. Among them, from the aspect of further improving the peeling performance of the chip component of the adhesive tape for semiconductor device manufacturing and further suppressing the residual glue to the chip component, it is preferably selected from at least one of carboxyl-containing monomers, hydroxyl-containing monomers, epoxy-containing monomers, double-bond-containing monomers, triple-bond-containing monomers and amide-containing monomers.

[0126] As the above-mentioned carboxyl-containing monomer, (meth) acrylic acid and other (meth) acrylic acid monomers can be mentioned. As the above-mentioned hydroxyl-containing monomer, hydroxyalkyl acrylates or hydroxyalkyl methacrylates such as (meth) acrylic acid 4-hydroxybutyl ester and (meth) acrylic acid 2-hydroxyethyl ester can be mentioned. As the above-mentioned epoxy-containing monomer, glycidyl (meth) acrylic acid can be mentioned. As the above-mentioned double-bond-containing monomer, allyl (meth) acrylic acid, hexanediol di(meth)acrylate, etc. can be mentioned. As the above-mentioned triple-bond-containing monomer, propargyl (meth) acrylic acid, etc. can be mentioned. As the above-mentioned amide-containing monomer, (meth) acrylamide, etc. can be mentioned. Among them, from the perspective of further improving the peeling performance of the chip component of the adhesive tape for semiconductor device manufacturing and further suppressing the residual glue to the chip component, carboxyl-containing monomers and hydroxyl-containing monomers are preferred. In addition, (meth) acrylic acid monomers and hydroxyalkyl acrylates are more preferred, and acrylic acid, 2-hydroxyethyl acrylate and 4-hydroxybutyl acrylate are further preferred.

[0127] In addition, the block A preferably also contains the structure derived from the crosslinkable functional group-containing monomer in addition to the block B.

[0128] In the above-mentioned ABA type block copolymer, the content of the structure derived from the monomer having a crosslinkable functional group (the total of the content in the above-mentioned block A and the content in the above-mentioned block B) is not particularly limited, and is preferably 0.1% by weight or more and 30% by weight or less. By making the content of the structure derived from the monomer having a crosslinkable functional group in the above-mentioned range, the cohesive force of the above-mentioned first adhesive layer is further improved, the peeling performance of the chip component of the adhesive tape for manufacturing semiconductor devices is further improved, and the residual glue to the chip component can be further suppressed. The more preferred lower limit of the content of the structure derived from the monomer having a crosslinkable functional group is 0.5% by weight, the more preferred lower limit is 1% by weight, the more preferred upper limit is 25% by weight, and the more preferred upper limit is 20% by weight.

[0129] In the above-mentioned ABA type block copolymer, the content of the above-mentioned block A (hard segment) is not particularly limited, preferably more than 1 weight % and less than 40 weight %. By making the content of the above-mentioned block A the above-mentioned range, the fracture strength of the above-mentioned first adhesive layer becomes higher, and the residual glue to the chip component can be further suppressed. The more preferred lower limit of the content of the above-mentioned block A is 2 weight %, the further preferred lower limit is 5 weight %, and the particularly preferred lower limit is 10 weight %. The more preferred upper limit of the content of the above-mentioned block A is 35 weight %, the further preferred upper limit is 30 weight %, the further preferred upper limit is 25 weight %, the further preferred upper limit is 22 weight %, and the particularly preferred upper limit is 20 weight %.

[0130] The weight average molecular weight (Mw) of the ABA type block copolymer is not particularly limited, preferably 50,000 or more and 800,000 or less. By making the weight average molecular weight the above range, it is easy to adjust the fracture strength, storage modulus G', gel fraction, etc. of the first adhesive layer to the range described later, and the peeling performance of the chip component of the semiconductor device manufacturing adhesive tape is further improved, and the residual glue to the chip component can be further suppressed. The more preferred lower limit of the weight average molecular weight is 75,000, the more preferred lower limit is 100,000, and the more preferred lower limit is 200,000. The more preferred upper limit of the weight average molecular weight is 600,000.

[0131] It should be noted that the weight average molecular weight can be obtained, for example, by GPC (Gel Permeation Chromatography) method in terms of standard polystyrene. More specifically, for example, the measurement can be performed using "2690 Separations Module" manufactured by Waters as a measuring device, "GPC KF-806L" manufactured by Showa Denko as a column, and ethyl acetate as a solvent, at a sample flow rate of 1 mL / min and a column temperature of 40°C.

[0132] The SP value of the ABA type block copolymer is not particularly limited, and is preferably 10 or less. By making the SP value below 10, it is possible to suppress the close fit with the chip component and further improve the peeling performance. The SP value is more preferably below 9.98, and more preferably below 9.95. The lower limit of the SP value is not particularly limited, but due to the difficulty of synthesis, so substantially about 8 is the lower limit.

[0133] It should be noted that the above-mentioned SP value is called a solubility parameter, which is a parameter used as an index of polarity. In this specification, the above-mentioned SP value is calculated using the Fedors method (RF Fedors, Polym. Eng. Sci., 14 (2), 147-154 (1974)). In addition, the SP value of the ABA type block copolymer can be calculated based on the SP value of each repeating unit in the copolymer using its mixing ratio (molar ratio).

[0134] In order to obtain the ABA type block copolymer, the raw material monomers of the block A and the block B are subjected to free radical reaction in the presence of a polymerization initiator to obtain the block A and the block B, respectively, and then the two are reacted or copolymerized. Alternatively, the raw material monomers of the block B may be added after the block A is obtained to carry out copolymerization.

[0135] As a method for carrying out the above-mentioned radical reaction, that is, a polymerization method, a conventionally known method can be used, for example, solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, etc. are mentioned.

[0136] The acrylic copolymer as a base polymer contained in the first pressure-sensitive adhesive layer is a copolymer having a structure derived from a (meth)acrylic monomer.

[0137] As the above-mentioned (meth) acrylic acid monomer, for example, the same monomer as the (meth) acrylic acid monomer in the above-mentioned ABA type block copolymer can be cited. Among them, from the viewpoint of balancing the peeling performance of chip components and the residual adhesive suppression effect on chip components, butyl (meth) acrylate and 2-ethylhexyl (meth) acrylate are preferred, and butyl acrylate and 2-ethylhexyl acrylate are more preferred.

[0138] The acrylic copolymer preferably further includes a structure derived from a crosslinkable functional group-containing monomer.

[0139] By making the acrylic copolymer contain the structure derived from the monomer containing crosslinkable functional groups, the cohesive force of the first adhesive layer is improved due to the crosslinking of the crosslinkable functional groups, so that the peeling performance of the chip components of the adhesive tape for manufacturing semiconductor devices is improved, and the residual glue on the chip components can be suppressed. The crosslinkable functional groups may be crosslinked or not, and crosslinking is more preferred. However, even if the uncrosslinked structure is maintained, the cohesive force of the first adhesive layer can be increased by the interaction between the functional groups, the peeling performance of the chip components of the adhesive tape for manufacturing semiconductor devices is improved, and the residual glue on the chip components can be suppressed.

[0140] Examples of the monomer having a crosslinkable functional group include the same monomers as those mentioned above for the monomer having a crosslinkable functional group in the ABA type block copolymer.

[0141] In the acrylic copolymer, the content of the structure derived from the monomer having a crosslinkable functional group is not particularly limited, and is preferably 0.1% by weight or more and 30% by weight or less. By making the content of the structure derived from the monomer having a crosslinkable functional group within the above range, the cohesive force of the first adhesive layer is further improved, the peeling performance of the chip components of the adhesive tape for semiconductor device manufacturing is further improved, and the residual adhesive on the chip components can be further suppressed. The more preferred lower limit of the content of the structure derived from the monomer having a crosslinkable functional group is 0.5% by weight, the more preferred lower limit is 1% by weight, the more preferred upper limit is 25% by weight, and the more preferred upper limit is 20% by weight.

[0142] The weight average molecular weight (Mw) of the acrylic copolymer is not particularly limited, but is preferably 200,000 to 2,000,000. By making the weight average molecular weight in the above range, it is easy to adjust the fracture strength, storage modulus G', gel fraction, etc. of the first adhesive layer to the range described later, and the peeling performance of the chip component of the adhesive tape for semiconductor device manufacturing is further improved, and the residual adhesive to the chip component can be further suppressed. The more preferred lower limit of the weight average molecular weight is 400,000, and the more preferred upper limit is 1,500,000.

[0143] The SP value of the acrylic copolymer is not particularly limited, but is preferably 10 or less. By making the SP value 10 or less, it is possible to suppress the close contact with the chip component and further improve the peeling performance. The SP value is more preferably 9.98 or less, and more preferably 9.95 or less. The lower limit of the SP value is not particularly limited, but due to the difficulty of synthesis, the lower limit is substantially about 8.

[0144] It should be noted that the above-mentioned SP value is called a solubility parameter, which is a parameter used as an index of polarity. In this specification, the calculation of the above-mentioned SP value uses the Fedors method (RF Fedors, Polym. Eng. Sci., 14 (2), 147-154 (1974)). In addition, the SP value of the acrylic copolymer can be calculated based on the SP value of each repeating unit in the copolymer using its mixing ratio (molar ratio).

[0145] The first pressure-sensitive adhesive layer preferably further contains a cross-linking agent.

[0146] The crosslinking agent is not particularly limited and is selected according to the type of the crosslinking functional group in the base polymer contained in the first adhesive layer, and examples thereof include isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, metal chelate crosslinking agents, etc. More specifically, for example, when the crosslinking functional group in the base polymer contained in the first adhesive layer is a carboxyl group, examples of the crosslinking agent include epoxy crosslinking agents, isocyanate crosslinking agents, metal chelate crosslinking agents, etc.

[0147] Among them, epoxy-based crosslinking agents and isocyanate-based crosslinking agents are preferred because they can easily adjust the breaking strength, storage elastic modulus G′, gel fraction, and the like of the first pressure-sensitive adhesive layer to the ranges described below.

[0148] The content of the crosslinking agent is not particularly limited, and the degree of crosslinking (gel fraction) of the first pressure-sensitive adhesive layer can be adjusted by adjusting the amount of crosslinkable functional groups in the base polymer contained in the first pressure-sensitive adhesive layer and the content of the crosslinking agent.

[0149] The content of the cross-linking agent is preferably 0.01 parts by weight or more and 10 parts by weight or less relative to 100 parts by weight of the base polymer contained in the first adhesive layer. By making the content of the cross-linking agent within the above range, the base polymer contained in the first adhesive layer can be appropriately cross-linked to increase the cohesive force of the first adhesive layer, and the peeling performance of the chip components of the adhesive tape for semiconductor device manufacturing is further improved, and the residual adhesive on the chip components can be further suppressed. The more preferred lower limit of the content of the cross-linking agent is 0.1 parts by weight, the more preferred upper limit is 5 parts by weight, the more preferred lower limit is 0.15 parts by weight, and the more preferred upper limit is 3 parts by weight.

[0150] The first pressure-sensitive adhesive layer may further contain a tackifier (adhesion-imparting agent).

[0151] The thickener may be a solid thickener at room temperature or a liquid thickener at room temperature. It should be noted that room temperature refers to 20 to 25° C. and liquid refers to having fluidity.

[0152] The tackifier is not particularly limited, and examples thereof include rosin ester resins, terpene phenol resins, terpene resins, and coumarone resins.

[0153] The content of the above-mentioned tackifier is not particularly limited. From the viewpoint of the peeling performance of the chip component of the adhesive tape for manufacturing semiconductor devices, it is preferably not contained in the above-mentioned first adhesive layer. In the case of containing the above-mentioned tackifier, it is preferably 10 parts by weight or less relative to 100 parts by weight of the base polymer contained in the above-mentioned first adhesive layer. By making the content of the above-mentioned tackifier within the above-mentioned range, the peeling performance of the chip component of the adhesive tape for manufacturing semiconductor devices is further improved. The more preferred upper limit of the content of the above-mentioned tackifier is 5 parts by weight.

[0154] The first adhesive layer may further contain the same ultraviolet absorber as that contained in the ablation layer within the range not impairing the effects of the present invention. The ultraviolet absorptivity of the first adhesive layer may be the same as that of the ablation layer, but is not particularly limited.

[0155] The first adhesive layer may further contain an inorganic filler such as fumed silica.

[0156] By adding the inorganic filler, the cohesive force of the first adhesive layer can be increased, the chip component peeling performance of the adhesive tape for semiconductor device manufacturing can be further improved, and the residual adhesive on the chip component can be further suppressed.

[0157] The first adhesive layer may further contain known additives such as a plasticizer, a resin, a surfactant, a wax, a particulate filler, etc. These additives may be used alone or in combination of two or more.

[0158] The fracture strength of the first adhesive layer is not particularly limited, and the preferred lower limit is 1 MPa. If the fracture strength is 1 MPa or more, the first adhesive layer is less likely to break when the chip component is peeled off by laser ablation, and the residual adhesive on the chip component can be further suppressed. The more preferred lower limit of the fracture strength is 1.3 MPa, and the further preferred lower limit is 1.4 MPa.

[0159] The upper limit of the above-mentioned breaking strength is not particularly limited. If the above-mentioned breaking strength is too high, the peeling performance of the chip components of the adhesive tape for semiconductor device manufacturing will be reduced. Therefore, the preferred upper limit is 10 MPa, the more preferred upper limit is 8 MPa, the further preferred upper limit is 7 MPa, and the further preferred upper limit is 6 MPa.

[0160] It should be noted that the breaking strength of the first adhesive layer can be calculated, for example, using Autograph (manufactured by Shimadzu Corporation) according to JIS K7161:2014, based on the stress at break when the adhesive layer is stretched at a stretching speed of 500 mm / min under an environment of a temperature of 23°C and a relative humidity of 50%. It should be noted that during the measurement, the first adhesive layer, etc., except for the first adhesive layer, is removed, and a sample consisting only of the first adhesive layer is prepared, and the breaking strength is measured. As a method for removing the substrate, etc., in order to avoid modification of the first adhesive layer, there is no particular limitation as long as treatment with a solvent, treatment with a chemical reaction, treatment at a high temperature, etc. is avoided. As a specific method, the following can be selected: after the first adhesive layers are bonded to each other, an appropriate temperature and peeling speed are selected and the layers are torn off, thereby removing the substrate, etc.; or a method of physically grinding the substrate, etc.

[0161] When the thickness of the first adhesive layer is less than 100 μm, the first adhesive layer is superposed to form an adhesive layer for measurement with a thickness of 100 μm or more. The breaking strength of the obtained adhesive layer for measurement is measured as described above.

[0162] The storage modulus (shear storage modulus) G' of the first adhesive layer at 23°C and 1 Hz is not particularly limited, but the preferred lower limit is 1×10 4 Pa, the upper limit of which is preferably 2×10 6 Pa. If the storage modulus G' is 1×10 4Pa or more, the peeling performance of the chip components of the adhesive tape for semiconductor device manufacturing is further improved. 6 Pa or less, the chip component holding performance of the adhesive tape for semiconductor device manufacturing is further improved. The more preferred lower limit of the storage elastic modulus G' is 2×10 4 Pa, and the more preferred upper limit is 1.5×10 6 Pa, and a further preferred lower limit is 3×10 4 Pa, and a further preferred upper limit is 1.2×10 6 Pa.

[0163] It should be noted that the storage modulus G' of the above-mentioned first adhesive layer at 23°C and 1 Hz can be obtained, for example, as the storage modulus at 23°C when a dynamic viscoelastic spectrum of -40 to 140°C is measured under the conditions of a heating rate of 5°C / min and 1 Hz in a simple heating mode using a viscoelastic spectrometer (manufactured by IT Measurement and Control Co., Ltd., DVA-200 or its equivalent).

[0164] When the thickness of the first adhesive layer is less than 100 μm, the first adhesive layer is superposed to form an adhesive layer for measurement with a thickness of 100 μm or more. The storage modulus G' of the obtained adhesive layer for measurement is measured as described above.

[0165] The storage modulus (shear storage modulus) G' of the first adhesive layer at -20°C and 1 Hz is not particularly limited, but the preferred lower limit is 3×10 5 Pa, the upper limit of which is preferably 1×10 8 Pa. If the storage modulus G' is 3×10 5 Pa or more, the peeling performance of the chip components of the adhesive tape for semiconductor device manufacturing is further improved. 8 Pa or less, the chip component holding performance of the adhesive tape for semiconductor device manufacturing is further improved. The more preferred lower limit of the storage elastic modulus G' is 5×10 6 Pa, and the more preferred upper limit is 5×10 7 Pa, and a further preferred lower limit is 1×10 7 Pa, and a further preferred upper limit is 3×10 7 Pa.

[0166] The storage modulus (shear storage modulus) G' of the first adhesive layer at 140°C and 1 Hz is not particularly limited, but the preferred lower limit is 3×10 4 Pa, the upper limit of which is preferably 3×10 5 Pa. If the storage modulus G' is 3×104 Pa or more, even when transferring chip components with protrusions or small-sized chip components, the chip component peeling performance of the adhesive tape for semiconductor device manufacturing is further improved. 5 Pa or less, the holding performance of the semiconductor device manufacturing adhesive tape with protruding chip components or small-sized chip components is further improved. The more preferred lower limit of the storage modulus G' is 5×10 4 Pa, and the more preferred upper limit is 2.5×10 5 Pa, and a further preferred lower limit is 9×10 4 Pa, and a further preferred upper limit is 2×10 5 Pa.

[0167] The storage modulus G' of the first adhesive layer at -20°C and 1 Hz and at 140°C and 1 Hz can be obtained, for example, as the storage modulus at -20°C and 140°C when a dynamic viscoelastic spectrum of -40 to 160°C is measured under the conditions of a heating rate of 5°C / min and 1 Hz in a simple heating mode using a viscoelastic spectrometer (manufactured by IT Measurement and Control Co., Ltd., DVA-200 or its equivalent).

[0168] When the thickness of the first adhesive layer is less than 100 μm, the first adhesive layer is superposed to form an adhesive layer for measurement with a thickness of 100 μm or more. The storage modulus G' of the obtained adhesive layer for measurement is measured as described above.

[0169] The gel fraction of the first adhesive layer is not particularly limited, but a preferred lower limit is 70% by weight, and a preferred upper limit is 95% by weight. If the gel fraction is 70% by weight or more, the peeling performance of the chip component of the adhesive tape for manufacturing semiconductor devices is further improved. If the gel fraction is 95% by weight or less, the holding performance of the chip component of the adhesive tape for manufacturing semiconductor devices is further improved. A more preferred lower limit of the gel fraction is 80% by weight, and a more preferred upper limit is 90% by weight.

[0170] In addition, the gel fraction of the above-mentioned first pressure-sensitive adhesive layer can be measured by the following method.

[0171] Only 0.1 g of the first adhesive layer (adhesive composition) was taken out from the adhesive tape for semiconductor device manufacturing, immersed in 50 mL of ethyl acetate, and shaken for 24 hours at a temperature of 23° C. and 200 rpm using a shaker. After shaking, the ethyl acetate and the adhesive composition swollen by absorbing the ethyl acetate were separated using a metal mesh (mesh #200 mesh). The separated adhesive composition was dried at 110° C. for 1 hour. The weight of the adhesive composition containing the metal mesh after drying was measured, and the gel fraction of the first adhesive layer was calculated using the following formula.

[0172] Gel fraction (wt%) = 100 × (W 1 -W 2 ) / W 0

[0173] (W 0 : Initial adhesive composition weight, W 1 : Weight of the adhesive composition containing the metal mesh after drying, W 2 : Initial weight of the metal mesh)

[0174] When the first adhesive composition cannot be completely dissolved in ethyl acetate, toluene, hexane, water or other solvents are used instead of ethyl acetate. Specifically, when the first adhesive composition contains a styrene elastomer, toluene or hexane is used, and when the first adhesive composition contains polyvinyl alcohol, hot water at 90° C. is used.

[0175] The method for adjusting the breaking strength, storage modulus G', gel fraction, etc. of the above-mentioned first adhesive layer to the above-mentioned range is not particularly limited, and examples thereof include: a method of adjusting the composition or weight average molecular weight (Mw) of the base polymer contained in the above-mentioned first adhesive layer, the type or amount of the above-mentioned cross-linking agent, etc.

[0176] The phase separation structure of the first adhesive layer is not particularly limited, and preferably has a spherical phase separation structure. By making the first adhesive layer have a spherical phase separation structure, it is easy to adjust the storage modulus, fracture strength, gel fraction, etc. of the first adhesive layer to the above range, the peeling performance of the chip component of the adhesive tape is further improved, and the residual adhesive to the chip component can be further suppressed. The phase separation structure of the first adhesive layer can be controlled, for example, by adjusting the ratio of each block in the ABA type block copolymer.

[0177] The first adhesive layer may also have a columnar phase separation structure. By making the first adhesive layer have a columnar phase separation structure, it is easy to adjust the storage modulus, fracture strength, gel fraction, etc. of the first adhesive layer to the above range, and the peeling performance of the chip component of the adhesive tape is further improved, and the residual glue on the chip component can be further suppressed. In particular, in the case where the first adhesive layer has a columnar phase separation structure, it is easy to adjust the storage modulus, fracture strength, etc. of the first adhesive layer to a larger range, even in the case of transferring a chip component with a protrusion or a small-sized chip component, the peeling performance of the chip component of the adhesive tape is further improved, and the residual glue on the chip component can be further suppressed.

[0178] The phase separation structure of the adhesive layer can be confirmed by transmission electron microscopy (TEM) observation. Spherical means that the microphase separation structure is a spherical structure, and columnar means that the microphase separation structure is a cylindrical structure.

[0179] In the case where the first adhesive layer has a spherical phase separation structure, the size of the island structure in the spherical phase separation structure is not particularly limited, and the preferred lower limit of the average major diameter of the island structure is 5 nm, the preferred upper limit is 100 nm, the more preferred lower limit is 10 nm, and the more preferred upper limit is 50 nm. By making the average major diameter within the above range, the peeling performance of the chip component of the adhesive tape is further improved, and the residual adhesive on the chip component can be further suppressed.

[0180] It should be noted that the average major diameter of the island structures in the spherical phase-separated structure can be measured by the following method.

[0181] The first adhesive layer was observed by transmission electron microscopy (TEM) at a magnification of 5000 times to obtain an observation image for an area of ​​4.3 μm × 4.3 μm. The obtained image was automatically binarized using image analysis software (e.g., Avizo, ver2019.4, manufactured by Thermo Fisher Scientific, etc.). The long diameter of each island structure (dark part) was measured based on the binarized image, and their arithmetic mean was taken as the average long diameter. It should be noted that the details of the automatic binarization method are based on known literature (“Automatic threshold selection method based on discrimination and least squares criteria”, Nobuyuki Otsu, Journal of the Institute of Electronics, Information and Communications Technology D, Vol. J63-D, No. 4, pp. 349-356).

[0182] The thickness of the first adhesive layer is not particularly limited, and the preferred lower limit is 3 μm, and the preferred upper limit is 50 μm. If the thickness of the first adhesive layer is 3 μm or more, the chip component holding performance and peeling performance of the adhesive tape for manufacturing semiconductor devices are further improved. If the thickness of the first adhesive layer is 50 μm or less, the residual adhesive on the chip components can be further suppressed. From the perspective of further improving the chip component holding performance and peeling performance of the adhesive tape for manufacturing semiconductor devices and further suppressing the residual adhesive on the chip components, the more preferred lower limit of the thickness of the first adhesive layer is 5 μm, the more preferred upper limit is 30 μm, the more preferred lower limit is 8 μm, and the more preferred upper limit is 20 μm.

[0183] The adhesive tape for manufacturing a semiconductor device of the present invention may include a second adhesive layer on the surface of the substrate opposite to the surface on which the ablation layer, the barrier layer, and the first adhesive layer are sequentially laminated.

[0184] That is, the adhesive tape for manufacturing a semiconductor device of the present invention may further include a second adhesive layer, and may include the second adhesive layer, the substrate, the ablation layer, the barrier layer, and the first adhesive layer in this order. If the second adhesive layer is included, the adhesive tape for manufacturing a semiconductor device of the present invention can be easily attached to a glass support or the like.

[0185] exist Figure 4 A cross-sectional view schematically showing an example of the adhesive tape for semiconductor device manufacturing of the present invention having the second adhesive layer is shown in FIG. Figure 4 In the adhesive tape 12 for manufacturing a semiconductor device of the present invention shown, the second adhesive layer 4b, the base material 5, the ablation layer 10, the barrier layer 11, and the first adhesive layer 4a are laminated in this order.

[0186] The second adhesive layer is not particularly limited, but is preferably a pressure-sensitive adhesive layer.

[0187] Examples of the base polymer contained in the second adhesive layer include ABA block copolymers, acrylic copolymers, urethane copolymers, silicone adhesives, etc. Among them, ABA block copolymers and acrylic copolymers are preferred from the viewpoint of being able to be firmly attached to a support such as a glass substrate and being able to be re-peeled without residual adhesive.

[0188] As the ABA block copolymer as the base polymer contained in the second pressure-sensitive adhesive layer, the same polymer as the ABA block copolymer used in the first pressure-sensitive adhesive layer can be used.

[0189] The phase separation structure of the second pressure-sensitive adhesive layer is not particularly limited, but is preferably a spherical phase separation structure from the viewpoint of achieving both strong adhesiveness and removability.

[0190] In the ABA type block copolymer, the block B is not particularly limited as long as it has a flexible structure. The block B preferably contains a structure derived from a (meth)acrylic acid monomer, and more preferably contains butyl acrylate or 2-ethylhexyl acrylate.

[0191] As the acrylic copolymer as the base polymer contained in the second pressure-sensitive adhesive layer, the same polymer as the acrylic copolymer used in the first pressure-sensitive adhesive layer can be used.

[0192] The acrylic copolymer as the base polymer contained in the second pressure-sensitive adhesive layer is a copolymer having a structure derived from a (meth)acrylic monomer.

[0193] Examples of the (meth)acrylic monomer include the same monomers as those in the ABA block copolymer, and among them, butyl acrylate and 2-ethylhexyl acrylate are more preferred from the viewpoint of achieving both strong adhesiveness and removability.

[0194] From the viewpoint of re-peeling without residual adhesive, the acrylic copolymer preferably contains a structure derived from a monomer having a crosslinkable functional group.

[0195] Examples of the monomer having a crosslinkable functional group include the same monomers as those mentioned above for the monomer having a crosslinkable functional group in the ABA type block copolymer.

[0196] In the acrylic copolymer, the content of the structure derived from the monomer having a crosslinkable functional group is not particularly limited, and is preferably 0.1% by weight or more and 30% by weight or less. By making the content of the structure derived from the monomer having a crosslinkable functional group within the above range, strong adhesion and re-peelability can be taken into account. The more preferred lower limit of the content of the structure derived from the monomer having a crosslinkable functional group is 0.5% by weight, the further preferred lower limit is 1% by weight, the more preferred upper limit is 25% by weight, and the further preferred upper limit is 20% by weight.

[0197] The weight average molecular weight (Mw) of the acrylic copolymer is not particularly limited, but is preferably 200,000 to 2,000,000. By making the weight average molecular weight in the above range, both strong adhesion and removability can be taken into account. The more preferred lower limit of the weight average molecular weight is 400,000, and the more preferred upper limit is 1,500,000.

[0198] The second pressure-sensitive adhesive layer preferably further contains a cross-linking agent.

[0199] The crosslinking agent is not particularly limited and is selected according to the type of the crosslinking functional group in the base polymer contained in the second adhesive layer, and examples thereof include isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, metal chelate crosslinking agents, etc. More specifically, for example, when the crosslinking functional group in the base polymer contained in the second adhesive layer is a carboxyl group, examples of the crosslinking agent include epoxy crosslinking agents, isocyanate crosslinking agents, metal chelate crosslinking agents, etc.

[0200] Among them, epoxy-based crosslinking agents and isocyanate-based crosslinking agents are preferred from the viewpoint of achieving both strong adhesiveness and removability.

[0201] The content of the crosslinking agent is not particularly limited, and the degree of crosslinking (gel fraction) of the second pressure-sensitive adhesive layer can be adjusted by adjusting the amount of crosslinkable functional groups in the base polymer contained in the second pressure-sensitive adhesive layer and the content of the crosslinking agent.

[0202] The content of the cross-linking agent is preferably 0.01 parts by weight or more and 10 parts by weight or less relative to 100 parts by weight of the base polymer contained in the second adhesive layer. By making the content of the cross-linking agent the above range, strong adhesion and re-peelability can be taken into account. The more preferred lower limit of the content of the cross-linking agent is 0.1 parts by weight, the more preferred upper limit is 5 parts by weight, the further preferred lower limit is 0.15 parts by weight, and the further preferred upper limit is 3 parts by weight.

[0203] The second pressure-sensitive adhesive layer may further contain a tackifier (adhesion-imparting agent).

[0204] The above-mentioned thickener is not particularly limited, and preferably has a moderate ultraviolet transmittance. The ultraviolet transmittance of the above-mentioned thickener is not particularly limited, and the preferred lower limit of the ultraviolet transmittance at a wavelength of 365nm is 1%, a more preferred lower limit is 50%, and a further preferred lower limit is 80%. The upper limit of the ultraviolet transmittance at the above-mentioned wavelength of 365nm is not particularly limited, and substantially about 95% is the upper limit. From the viewpoint of high ultraviolet transmittance, a hydrogenated thickener is preferred.

[0205] The tackifier is not particularly limited, and examples thereof include rosin ester resins, terpene phenol resins, terpene resins, coumarone resins, etc. Among them, hydrogenated rosin esters, hydrogenated terpene phenols, hydrogenated terpene resins, etc. are preferred.

[0206] The content of the above-mentioned tackifier is not particularly limited, and from the viewpoint of re-peelability, it is preferably not contained in the above-mentioned second adhesive layer. When containing the above-mentioned tackifier, relative to 100 weight parts of the base polymer contained in the above-mentioned second adhesive layer, it is preferably less than 10 weight parts. If the content of the solid tackifier at the above-mentioned room temperature is the above-mentioned range, it is not easy to produce residual glue when peeling again. The more preferred lower limit of the content of the above-mentioned tackifier is 5 weight parts, and the more preferred upper limit is 3 weight parts.

[0207] The second adhesive layer preferably has a moderate ultraviolet transmittance. The ultraviolet transmittance is not particularly limited, and the preferred lower limit of the ultraviolet transmittance at a wavelength of 365 nm is 1%, a more preferred lower limit is 50%, and a further preferred lower limit is 80%. The upper limit of the ultraviolet transmittance at a wavelength of 365 nm is not particularly limited, and substantially about 95% is the upper limit.

[0208] The second adhesive layer may further contain an inorganic filler such as fumed silica.

[0209] By adding the inorganic filler, the cohesive force of the second adhesive is improved, and it is easy to achieve both strong adhesiveness and removability.

[0210] The second pressure-sensitive adhesive layer may further contain known additives such as a plasticizer, a resin, a surfactant, a wax, a particulate filler, etc. These additives may be used alone or in combination of two or more.

[0211] The adhesive force of the second adhesive layer is not particularly limited, but the preferred lower limit is 0.8 N / 25 mm. If the adhesive force is 0.8 N / 25 mm or more, it is possible to prevent the adhesive tape from peeling off from a support such as a glass substrate when peeling off the chip component. The more preferred lower limit of the adhesive force is 2 N / 25 mm, the further preferred lower limit is 6 N / 25 mm, and the further preferred lower limit is 12 N / 25 mm.

[0212] The upper limit of the adhesive strength is not particularly limited, but from the viewpoint of removability, the upper limit is preferably 20 N / 25 mm, the upper limit is more preferably 18 N / 25 mm, and the upper limit is still more preferably 16 N / 25 mm.

[0213] It should be noted that the adhesive strength of the above-mentioned second adhesive layer is obtained, for example, by the following method: using Autograph (manufactured by Shimadzu Corporation), etc., the adhesive tape is cut into 25 mm wide according to JIS Z0237:2009, and is attached to a glass plate at a speed of 300 mm / min using a 2 kg crimping rubber roller at room temperature of 23°C and a relative humidity of 50%. After leaving it for 30 minutes, the adhesive tape is torn off at a speed of 300 mm / min, and the 180° peel strength is measured.

[0214] The gel fraction of the second adhesive layer is not particularly limited, and a preferred lower limit is 30% by weight, and a preferred upper limit is 90% by weight. If the gel fraction is more than 30% by weight, it is difficult to produce residual glue when peeling off again. If the gel fraction is below 90% by weight, it is easy to adjust the adhesive force to be high. A more preferred lower limit of the gel fraction is 40% by weight, and a more preferred upper limit is 80% by weight.

[0215] In addition, the gel fraction of the second pressure-sensitive adhesive layer can be measured by the following method.

[0216] Only 0.1 g of the second adhesive layer (adhesive composition) was taken out from the adhesive tape for semiconductor device manufacturing, immersed in 50 mL of ethyl acetate, and shaken for 24 hours at a temperature of 23° C. and 200 rpm using a shaker. After shaking, the ethyl acetate and the adhesive composition swollen by absorbing the ethyl acetate were separated using a metal mesh (mesh #200 mesh). The separated adhesive composition was dried at 110° C. for 1 hour. The weight of the adhesive composition containing the metal mesh after drying was measured, and the gel fraction of the second adhesive layer was calculated using the following formula.

[0217] Gel fraction (wt%) = 100 × (W 1 -W 2 ) / W 0

[0218] (W 0 : Initial adhesive composition weight, W 1 : Weight of the adhesive composition containing the metal mesh after drying, W 2 : Initial weight of the metal mesh)

[0219] When the second adhesive composition cannot be completely dissolved in ethyl acetate, toluene, hexane, water or other solvents are used instead of ethyl acetate. Specifically, when the second adhesive composition contains a styrene elastomer, toluene or hexane is used, and when the second adhesive composition contains polyvinyl alcohol, hot water at 90° C. is used.

[0220] The method for adjusting the adhesive force, gel fraction, etc. of the above-mentioned second adhesive layer to the above-mentioned range is not particularly limited, and examples thereof include: a method of adjusting the composition or weight average molecular weight (Mw) of the base polymer contained in the above-mentioned second adhesive layer, the type or amount of the above-mentioned cross-linking agent, etc.

[0221] The thickness of the second adhesive layer is not particularly limited, and the preferred lower limit is 3 μm, and the preferred upper limit is 30 μm. If the thickness of the second adhesive layer is 3 μm or more, it is possible to prevent the adhesive tape from being peeled off from a support such as a glass substrate when the chip component is peeled off. If the thickness of the second adhesive layer is 30 μm or less, it can be easily peeled off again. The more preferred lower limit of the thickness of the second adhesive layer is 5 μm, the more preferred upper limit is 20 μm, the further preferred lower limit is 8 μm, and the further preferred upper limit is 12 μm.

[0222] The adhesive tape for semiconductor device manufacturing of the present invention only needs to have the substrate, ablation layer, barrier layer and first adhesive layer in sequence as described above, and may further have other layers within the scope that does not impair the effect of the present invention. In the case where the barrier layer has an easy-adhesion resin layer on the surface in contact with the first adhesive layer, it only needs to have the substrate, ablation layer, barrier layer (having an easy-adhesion resin layer on the surface in contact with the first adhesive layer) and first adhesive layer in sequence as described above, and may further have other layers within the scope that does not impair the effect of the present invention. In the case of having the second adhesive layer, it only needs to have the second adhesive layer, substrate, ablation layer, barrier layer and first adhesive layer in sequence, and may further have other layers within the scope that does not impair the effect of the present invention.

[0223] The rolling ball tack of the first adhesive layer of the adhesive tape for manufacturing semiconductor devices of the present invention is not particularly limited, but is preferably No. 5 or above. If the rolling ball tack is No. 5 or above, the chip component retention performance of the adhesive tape for manufacturing semiconductor devices is further improved. The rolling ball tack is more preferably No. 6 or above. The upper limit of the rolling ball tack is not particularly limited, but is preferably No. 12 or below from the viewpoint of further improving the peeling performance of the chip components.

[0224] The rolling ball tack of the pressure-sensitive adhesive tape for semiconductor device manufacturing can be calculated, for example, by measuring the rolling ball tack in an environment of 23° C. and 50% relative humidity in accordance with JIS Z0237 using a rolling ball tack tester (manufactured by Yasuda Seiki Co., Ltd.).

[0225] The surface peeling force of the first adhesive layer of the semiconductor device manufacturing adhesive tape of the present invention is not particularly limited, and the preferred upper limit is 1MPa. If the above-mentioned surface peeling force is below 1MPa, the peeling performance of the chip component of the semiconductor device manufacturing adhesive tape is further improved. The more preferred upper limit of the above-mentioned surface peeling force is 0.8MPa. The lower limit of the above-mentioned surface peeling force is not particularly limited, and from the viewpoint of further improving the holding performance of the chip component, the preferred lower limit is 0.65MPa.

[0226] It should be noted that the surface peeling force of the first adhesive layer of the adhesive tape for semiconductor device manufacturing can be obtained as follows. One side of a cube made of SUS with a side of 10 mm is attached to the surface of the first adhesive layer of the adhesive tape for semiconductor device manufacturing, and is crimped with 0.3 MPa for 10 seconds under a temperature of 23 ° C and a relative humidity of 50%. Then, using Autograph (made by Shimadzu Corporation) or the like, the cube made of SUS is stretched at a tension rate of 1000 mm / min under a temperature of 23 ° C and a relative humidity of 50% to be peeled off while the substrate surface of the adhesive tape for semiconductor device manufacturing is fixed. The maximum stress during peeling is taken as the surface peeling force.

[0227] The visible light transmittance of the adhesive tape for semiconductor device manufacturing of the present invention is not particularly limited, and preferably has a moderate visible light transmittance from the viewpoint of peeling off chip components by laser ablation. The preferred lower limit of the above-mentioned visible light transmittance is 50%, and the more preferred lower limit is 80%. The upper limit of the above-mentioned visible light transmittance is not particularly limited, and substantially about 95% is the upper limit.

[0228] The haze of the adhesive tape for semiconductor device manufacturing of the present invention is not particularly limited, but from the viewpoint of peeling off chip components by laser ablation, the haze is preferably small. The preferred upper limit of the haze is 10%, the more preferred upper limit is 5%, and the further preferred upper limit is 3%. The lower limit of the haze is not particularly limited, but the smaller the haze, the more preferred it is. The actual lower limit is about 0.1%.

[0229] In addition, the visible light transmittance and haze of the pressure-sensitive adhesive tape for semiconductor device manufacturing can be measured using, for example, a haze meter (NDH4000, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0230] The use of the adhesive tape for semiconductor device manufacturing of the present invention is not particularly limited, and is suitable for use in the manufacture of semiconductor devices having a laser irradiation process. The adhesive tape for semiconductor device manufacturing of the present invention is more suitable for use in the manufacture of semiconductor devices having a laser irradiation process because it has excellent chip component peeling performance and can suppress residual adhesive on chip components. Figure 3 The step of peeling off the chip components arranged on the first adhesive layer by laser ablation as shown.

[0231] The chip component is not particularly limited, and examples thereof include MiniLED chips, microLED chips, optical chips of image sensors, and the like, with microLED chips being particularly preferred.

[0232] There is no particular limitation on the method for transferring chip components using the adhesive tape for manufacturing semiconductor devices of the present invention. For example, there can be cited a method for transferring chip components including the following steps: a step of arranging chip components on the first adhesive layer of the adhesive tape for manufacturing semiconductor devices of the present invention; and a step of irradiating the chip components with laser to peel off the chip components. In addition, there is no particular limitation on the method for manufacturing electronic device components using the adhesive tape for manufacturing semiconductor devices of the present invention. For example, there can be cited a method for manufacturing electronic device components including the above-mentioned method for transferring chip components. According to these methods, chip components can be transferred with a good yield, and residual adhesive on chip components can be suppressed.

[0233] Effects of the Invention

[0234] According to the present invention, it is possible to provide an adhesive tape for semiconductor device manufacturing that is excellent in chip component peeling performance and can suppress adhesive residue on chip components. BRIEF DESCRIPTION OF THE DRAWINGS

[0235] Figure 1 This is a cross-sectional view schematically showing an example of a process of peeling off chip components arranged on an adhesive layer by laser ablation using a conventional adhesive tape.

[0236] Figure 2 This is a cross-sectional view schematically showing an example of the adhesive tape for manufacturing a semiconductor device of the present invention.

[0237] Figure 3 This is a cross-sectional view schematically showing an example of a process of peeling off chip components arranged on the first adhesive layer by laser ablation using the adhesive tape for manufacturing a semiconductor device of the present invention.

[0238] Figure 4 This is a cross-sectional view schematically showing an example of the adhesive tape for manufacturing a semiconductor device of the present invention when having a second adhesive layer. DETAILED DESCRIPTION

[0239] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0240] (Adhesive A)

[0241] (1) Preparation of acrylic copolymer (1)

[0242] 52 parts by weight of ethyl acetate were placed in a reactor equipped with a thermometer, a stirrer, and a condenser. After nitrogen substitution, the reactor was heated and refluxed. 0.08 parts by weight of azobisisobutyronitrile was added as a polymerization initiator 30 minutes after the ethyl acetate began to boil. A monomer mixture containing 98 parts by weight of butyl acrylate (BA) and 2 parts by weight of acrylic acid (AAc) was uniformly and slowly added dropwise over 1 hour and 30 minutes to react. 0.1 parts by weight of azobisisobutyronitrile was added 30 minutes after the addition was completed, and the polymerization reaction was further carried out for 5 hours. Ethyl acetate was added to the reactor to dilute it while cooling it, thereby obtaining a solution of an acrylic copolymer (1) with a solid content of 30% by weight.

[0243] The weight average molecular weight of the obtained acrylic copolymer (1) was measured by GPC method. The measurement was performed using "2690 Separations Module" manufactured by Waters as a measuring device, "GPC KF-806L" manufactured by Showa Denko K.K. as a column, and ethyl acetate as a solvent, under the conditions of a sample flow rate of 1 mL / min and a column temperature of 40°C.

[0244] In addition, for the obtained acrylic copolymer (1), the SP value of the entire polymer was calculated by the Fedors method.

[0245] (2) Preparation of adhesive solution

[0246] The obtained acrylic copolymer (1) was dissolved in ethyl acetate so that the solid content was 15% by weight. 3.6 parts by weight of Coronate L (manufactured by Tosoh Corporation) as an isocyanate crosslinking agent and 8 parts by weight of Tinuvin 928 (manufactured by BASF Japan, a benzotriazole-based ultraviolet absorber) were added to 100 parts by weight of the acrylic copolymer (1), and the mixture was further stirred sufficiently to obtain an adhesive solution of an adhesive A.

[0247] (Adhesive B)

[0248] (1) Preparation of ABA type block copolymer (1)

[0249] In an autoclave, 500 parts by weight of degassed and dehydrated cyclohexane, 0.13 parts by weight of n-butyl lithium (n-BuLi) and tetrahydrofuran (THF) were added at a molar ratio of n-BuLi / THF = 40. Next, 4.5 parts by weight of styrene monomer was added and polymerization was carried out at 40°C to obtain a copolymer (block A). After the polymerization conversion rate of the styrene monomer reached about 100%, 91 parts by weight of 1,3-butadiene monomer was added for polymerization to obtain an AB type block copolymer. After the polymerization conversion rate reached approximately 100%, 4.5 parts by weight of styrene monomer was further added and polymerization was carried out at 40°C until the polymerization conversion rate reached about 100%, to obtain an ABA type block copolymer (before hydrogenation).

[0250] The ABA type block copolymer was diluted with purified and dried cyclohexane to adjust the polymer concentration to 5% by weight and subjected to a hydrogenation reaction. The hydrogenation reaction was started with a hydrogen supply pressure of 0.7 MPa-Gauge and a reaction temperature of 80°C under stirring. When the absorption of hydrogen was completed, the reaction solution was returned to normal temperature and pressure and taken out from the reaction vessel, thereby obtaining an ABA type block copolymer (1).

[0251] The weight average molecular weight of the obtained ABA type block copolymer (1) was measured by GPC method. It should be noted that the measurement was performed using "2690 Separations Module" manufactured by Waters as a measuring device, "GPC KF-806L" manufactured by Showa Denko K.K. as a column, and ethyl acetate as a solvent, under the conditions of a sample flow rate of 1 mL / min and a column temperature of 40°C.

[0252] In addition, for the obtained ABA type block copolymer (1), the glass transition temperature of block B was determined using the value obtained in the second run when the measurement was carried out under a nitrogen atmosphere and a heating rate of 10°C / min using a differential scanning calorimeter (SII Exstar 6000 / DSC6220 manufactured by Hitachi High-Tech Science Co., Ltd.). It should be noted that a peak derived from block A and a peak derived from block B were obtained, and the peak on the low temperature side was regarded as a peak derived from block B, and the glass transition temperature of block B was determined.

[0253] In addition, for the obtained ABA type block copolymer (1), according to 1 The ratio of ethylene to butene was calculated from the peak area ratio of ethylene and butene components measured by H-NMR, and the SP values ​​of the entire polymer and block B were calculated by the Fedors method.

[0254] (2) Preparation of adhesive solution

[0255] The obtained ABA type block copolymer (1) was dissolved in toluene so that the solid content was 20 wt%. 8 wt parts of Tinuvin 928 (benzotriazole type ultraviolet absorber manufactured by BASF Japan) was added as an ultraviolet absorber to 100 wt parts of the ABA type block copolymer (1), and the mixture was further stirred to obtain an adhesive solution of adhesive B.

[0256] (3) Confirmation of phase separation structure

[0257] Only the adhesive layer was prepared using the same method as in the examples and comparative examples described later. The small pieces obtained by cutting the adhesive layer were dyed with a 2% osmium acid aqueous solution at 60°C for 12 hours and then washed. A cryo-microtome (LEICA, ULTRACUT FC7) was used to cut the adhesive layer at a temperature of -100°C along the thickness direction of the small piece, and a slice having a thickness of less than 100 nm was cut out. The cut slices were placed on a sheet mesh (Japanese: シートメッシュ) with a support film as a measurement sample. The obtained measurement sample was observed using a transmission electron microscope (JEOL, JEM-2100) at a magnification of 5000 times, and the phase separation structure was confirmed, and the result showed a spherical phase separation structure.

[0258] (Adhesive C)

[0259] (1) Preparation of ABA type block copolymer (2)

[0260] 0.902 g of 1,6-hexanedithiol, 1.83 g of carbon disulfide and 11 mL of dimethylformamide were placed in a two-necked flask and stirred at 25°C. 2.49 g of triethylamine was added dropwise over 15 minutes and stirred at 25°C for 3 hours. Next, 2.75 g of methyl-α-bromophenylacetic acid was added dropwise over 15 minutes and stirred at 25°C for 4 hours. Then, 100 mL of an extraction solvent (n-hexane: ethyl acetate = 50:50) and 50 mL of water were added to the reaction solution for liquid separation extraction. The organic layers obtained by the first and second liquid separation extractions were mixed and washed with 50 mL of 1M hydrochloric acid, 50 mL of water, and 50 mL of saturated brine in sequence. Sodium sulfate was added to the washed organic layer for drying, and the sodium sulfate was filtered, and the filtrate was concentrated by an evaporator to remove the organic solvent. The obtained concentrate was purified by silica gel column chromatography to obtain a RAFT agent.

[0261] 15 parts by weight of styrene (St), 2 parts by weight of acrylic acid (AAc), 1.9 parts by weight of a RAFT agent, and 2,2'-azobis(2-methylbutyronitrile) (ABN-E) were placed in a two-necked flask, and the temperature was raised to 85° C. while replacing the inside of the flask with nitrogen. Then, the mixture was stirred at 85° C. for 6 hours to perform a polymerization reaction (first stage reaction).

[0262] After the reaction, 4000 parts by weight of n-hexane was added to the flask and stirred to precipitate the reactant. Unreacted monomers and RAFT agent were filtered and the reactant was dried under reduced pressure at 70° C. to obtain a copolymer (block A).

[0263] A mixture containing 81 parts by weight of butyl acrylate (BA), 2 parts by weight of acrylic acid (AAc), 0.058 parts by weight of ABN-E and 50 parts by weight of ethyl acetate, and the copolymer (block A) obtained above were placed in a two-necked flask, and the temperature was raised to 85° C. while the inside of the flask was replaced with nitrogen. Then, a polymerization reaction (second stage reaction) was carried out at 85° C. with stirring for 6 hours to obtain a reaction solution containing a block copolymer composed of block A and block B.

[0264] A portion of the reaction solution was collected, 4000 parts by weight of n-hexane was added thereto, and the mixture was stirred to precipitate the reactant. Unreacted monomers and solvent were filtered out, and the reactant was dried under reduced pressure at 70° C. to obtain an ABA type block copolymer (2).

[0265] The weight average molecular weight of the obtained ABA block copolymer (2) was measured by GPC method. It should be noted that the measurement was performed using "2690 Separations Module" manufactured by Waters as a measuring device, "GPC KF-806L" manufactured by Showa Denko K.K. as a column, and ethyl acetate as a solvent, under the conditions of a sample flow rate of 1 mL / min and a column temperature of 40°C.

[0266] In addition, for the obtained ABA type block copolymer (2), the glass transition temperature of block B was determined using the value obtained in the second run when the measurement was carried out under a nitrogen atmosphere and a heating rate of 10°C / min using a differential scanning calorimeter (SII Exstar 6000 / DSC6220 manufactured by Hitachi High-Tech Science Co., Ltd.). It should be noted that a peak derived from block A and a peak derived from block B were obtained, and the peak on the low temperature side was regarded as a peak derived from block B, and the glass transition temperature of block B was determined.

[0267] In addition, for the obtained ABA type block copolymer (2), the SP values ​​of the entire polymer and the block B were calculated by the Fedors method.

[0268] (2) Preparation of adhesive solution

[0269] The obtained ABA type block copolymer (2) was dissolved in ethyl acetate so that the solid content was 15 wt%. 1 part by weight of TETRAD C (manufactured by Mitsubishi Chemical Corporation) as an epoxy crosslinking agent and 8 parts by weight of Tinuvin 928 (manufactured by BASF Japan, a benzotriazole type ultraviolet absorber) as an ultraviolet absorber were added to 100 parts by weight of the ABA type block copolymer (2), and the mixture was further stirred sufficiently to obtain an adhesive solution of an adhesive C.

[0270] (3) Confirmation of phase separation structure

[0271] Only the adhesive layer was prepared using the same method as in the examples and comparative examples described later. The small pieces obtained by cutting the adhesive layer were stained with a 2% osmium acid aqueous solution at 60°C for 12 hours and then washed. A low-temperature microtome (LEICA, ULTRACUT FC7) was used to cut the adhesive layer at a small piece temperature of -100°C in the thickness direction, and slices with a thickness of less than 100nm were cut out. The cut slices were placed on a sheet net with a support film as measurement samples. The obtained measurement sample was observed using a transmission electron microscope (JEOL, JEM-2100) at a magnification of 5000 times, and the phase separation structure was confirmed, and the result showed a spherical phase separation structure.

[0272] (Adhesives D to E, J to O and R)

[0273] A pressure-sensitive adhesive solution was obtained in the same manner as in the pressure-sensitive adhesive C except that the composition of the ABA block copolymer, the type or amount of the ultraviolet absorber, and the type or amount of the cross-linking agent were changed as shown in Tables 1 and 2.

[0274] (Adhesives F to I, P and Q)

[0275] The same procedure as in Adhesive A was followed to obtain an adhesive solution except that the composition of the acrylic copolymer, the type or amount of the ultraviolet absorber, and the type or amount of the crosslinking agent were changed as shown in Tables 1 and 2. In Adhesive H, Tinuvin 460 (a hydroxyphenyltriazine ultraviolet absorber manufactured by BASF Japan) was used as the ultraviolet absorber.

[0276] The letter symbols in the table represent the following abbreviations.

[0277] St:Styrene

[0278] AAc: Acrylic acid

[0279] BA: Butyl acrylate

[0280] 2-EHA: 2-Ethylhexyl acrylate

[0281] LA: Lauryl acrylate

[0282] MA: Methyl acrylate

[0283] MOEA: Methoxyethyl acrylate

[0284] 2-HEA: 2-Hydroxyethyl acrylate

[0285]

[0286]

[0287] (Example 1)

[0288] (1) Manufacturing of adhesive tape

[0289] The obtained adhesive solution of adhesive A was applied to a corona-treated polyethylene terephthalate (PET) film with a thickness of 50 μm and a haze of 3.8% as a substrate using an applicator so that the thickness of the dry film became 16 μm, and dried at 110° C. for 3 minutes to form an ablation layer. This was used as a laminate film (a). Next, the ablation layer side of the laminate film (a) was overlapped with a corona-treated PET film with a thickness of 4 μm as a barrier layer. This was used as a laminate film (b).

[0290] On the other hand, the adhesive solution of the obtained adhesive A was applied to the release-treated surface of a 75 μm release PET film treated with a release agent using an applicator so that the dry film thickness was 10 μm, and dried at 110° C. for 3 minutes to form an adhesive layer. The adhesive layer was bonded to the barrier layer side of the laminated film (b). Then, it was heated and aged at 40° C. for 48 hours to obtain an adhesive tape having a substrate, an ablation layer, a barrier layer, a first adhesive layer, and a release PET film in this order.

[0291] (2) Measurement of breaking strength of first adhesive layer

[0292] A sheet with a thickness of 500 μm consisting only of the first adhesive layer was prepared. The breaking strength of the adhesive layer was calculated from the stress at break when stretched at a rate of 500 mm / min at a temperature of 23° C. and a relative humidity of 50% using Autograph (manufactured by Shimadzu Corporation) in accordance with JIS K7161.

[0293] (3) Measurement of Gel Fraction of First Adhesive Layer and Ablation Layer

[0294] Take out only 0.1 g of the first adhesive layer (adhesive composition) and only 0.1 g of the ablation layer (ablation layer composition) from the adhesive tape, immerse them in 50 mL of ethyl acetate respectively, and shake them for 24 hours at 23°C and 200 rpm using a shaker. After shaking, separate the ethyl acetate and the composition that has swollen due to absorption of ethyl acetate using a metal mesh (mesh size #200). Dry the separated composition at 110°C for 1 hour. Measure the weight of the composition containing the metal mesh after drying respectively, and calculate the gel fraction of the first adhesive layer and the ablation layer using the following formula.

[0295] Gel fraction (wt%) = 100 × (W 1 -W 2 ) / W 0

[0296] (W 0 : Initial composition weight, W 1 : Weight of the composition containing the metal mesh after drying, W 2 : Initial weight of the metal mesh)

[0297] In addition, the gel fractions of the ablation layer of Example 3 and the first adhesive layer of Example 4 were measured using toluene instead of ethyl acetate.

[0298] (4) Measurement of the storage modulus (shear storage modulus) G' of the ablation layer at 23°C and 1 Hz and the storage modulus (shear storage modulus) G' of the first adhesive layer at -20°C, 23°C, 140°C and 1 Hz

[0299] Separately, a sheet with a thickness of 1 mm consisting of only the ablation layer or the first adhesive layer was prepared. For the ablation layer and the first adhesive layer, the storage modulus G' at -20°C, 23°C, and 140°C was determined when the dynamic viscoelastic spectrum of -40 to 160°C was measured under the conditions of a heating rate of 5°C / min and 1 Hz in a simple heating mode using a viscoelastic spectrometer DVA-200 (manufactured by IT Instrumentation and Control Co., Ltd.).

[0300] (5) Measurement of UV Absorption of Ablation Layer and First Adhesive Layer

[0301] The ultraviolet absorptivity of the ablative layer and the first adhesive layer at a wavelength of 365 nm was measured using a spectrophotometer (UV-2600i, manufactured by Shimadzu Corporation) in accordance with JIS L1925.

[0302] (6) Determination of rolling ball initial adhesion of adhesive tape

[0303] The pressure-sensitive adhesive tape was measured for rolling ball tack using a rolling ball tack tester (manufactured by Yasuda Seiki Co., Ltd.) in accordance with JIS Z0237 under an environment of a temperature of 23° C. and a relative humidity of 50%.

[0304] (7) Surface peeling strength of the first adhesive layer of the adhesive tape

[0305] For the adhesive tape, a 10 mm SUS cube was attached to the surface of the first adhesive layer of the adhesive tape, and the tape was crimped at 0.3 MPa for 10 seconds at a temperature of 23°C and a relative humidity of 50%. Then, using Autograph (made by Shimadzu Corporation), the SUS cube was stretched at a tension rate of 1000 mm / min under a temperature of 23°C and a relative humidity of 50% to peel it off. The maximum stress during the peeling was measured as the surface peeling force.

[0306] (Examples 2 to 18, 22 to 24, Comparative Examples 1 to 4)

[0307] The adhesive tapes were obtained in the same manner as in Example 1 except that each layer was changed as shown in Tables 3, 4 and 5. In Examples 15 to 18 and 22 to 24, a PET film having a thickness of 50 μm and a haze of 0.3% was used as the substrate, and a PET film having a thickness of 5.5 μm and an easy-adhesion resin layer (the elastic modulus of the easy-adhesion resin layer by nanoindentation method was 5850 MPa) was used as the barrier layer.

[0308] (Example 19)

[0309] (1) Production of double-sided adhesive tape

[0310] The obtained adhesive solution of the adhesive P was applied to a polyethylene terephthalate film having one surface subjected to a release treatment using an applicator so that the dry film thickness was 10 μm, and dried at 110° C. for 3 minutes to prepare a laminated film (p) having an adhesive layer on the release-treated surface of the polyethylene terephthalate film.

[0311] Next, an adhesive tape was prepared in the same manner as in Example 1 except that each layer was changed as shown in Table 4, and a laminated film (p) was laminated from the adhesive layer surface on the side of the substrate of the obtained adhesive tape opposite to the side on which the ablative layer, the barrier layer, the first adhesive layer, and the release PET film were laminated in sequence, and the adhesive layer was transferred to the substrate and laminated integrally. Thus, a double-sided adhesive tape having a second adhesive layer having the thickness and gel fraction shown in Table 4 was obtained.

[0312] The following items are measured using the same method as in Example 1: the breaking strength of the first adhesive layer, the gel fraction of the first adhesive layer and the ablation layer, the storage modulus (shear storage modulus) G' of the ablation layer at 23°C and 1 Hz and the storage modulus (shear storage modulus) G' of the first adhesive layer at -20°C, 23°C, 140°C and 1 Hz, the ultraviolet absorptivity of the ablation layer and the first adhesive layer, the rolling ball initial adhesion of the adhesive tape, and the surface peeling force of the first adhesive layer of the adhesive tape.

[0313] The gel fraction of the second adhesive layer was measured by the same method as in the above-mentioned "(3) Measurement of gel fraction of first adhesive layer and ablation layer".

[0314] (Examples 20, 21)

[0315] Except having changed each layer as shown in Table 4, it carried out similarly to Example 19, and obtained the adhesive tape.

[0316] (2) Adhesive strength of the second adhesive layer of the adhesive tape

[0317] The double-sided adhesive tape obtained by the above method was cut into 25 mm wide, and a PET film of 25 μm of thickness cut into 30 mm wide was attached to the surface of the first adhesive layer of the double-sided adhesive tape. Then, at room temperature 23°C and relative humidity 50%, a 2 kg crimping rubber roller was used to attach the surface of the second adhesive layer to a glass plate at a speed of 300 mm / min. Then, using Autograph (Shimadzu Corporation), at a temperature of 23°C and a relative humidity of 50%, the second adhesive layer side of the double-sided adhesive tape was torn off at a speed of 300 mm / min along a 180° direction, and the 180° adhesive force was measured.

[0318] <Evaluation>

[0319] The pressure-sensitive adhesive tapes obtained in Examples and Comparative Examples were evaluated as follows.

[0320] (1) Laser ablation evaluation

[0321] (1-1-1) Chip component retention and peeling performance

[0322] The obtained adhesive tape was attached to the surface of the Si chip side of a wafer on which 10 Si chips (500 μm×500 μm square, 50 μm thickness) were arranged. Then, the Si chip was arranged on the adhesive tape by peeling off the wafer. A semiconductor solid-state laser was used to irradiate each Si chip with a 365 nm laser having an output power of 4 W and 4 kHz from the substrate side of the adhesive tape to peel off the Si chip from the adhesive tape.

[0323] The case where all Si chips can be configured on the adhesive tape from the wafer is marked as "○", the case where 8 to 9 Si chips can be configured on the adhesive tape is marked as "△", and the case where less than 7 Si chips can be configured on the adhesive tape is marked as "×" to evaluate the retention performance of the chip components.

[0324] The peeling performance of the chip components was evaluated by setting the case where all 10 Si chips could be peeled off from the adhesive tape as "◎", the case where 8 to 9 Si chips could be peeled off from the adhesive tape as "○", the case where 7 Si chips could be peeled off from the adhesive tape as "△", and the case where 6 or less Si chips could be peeled off from the adhesive tape as "×". In the case where the adhesive tape has a second adhesive layer, the evaluation was performed in a state where the second adhesive layer was attached to a glass support having a thickness of 2 mm.

[0325] (1-1-2) Residual Glue

[0326] After evaluating the holding performance and peeling performance of the chip components, the surface of the Si chip peeled from the adhesive tape was observed under a microscope to confirm whether there was residual adhesive. The case where there was no residual adhesive was set as "◎", the case where less than 20% of the surface area of ​​the chip component had residual adhesive was set as "0", and the case where more than 20% of the surface area of ​​the chip component had residual adhesive was set as "×" to evaluate the residual adhesive.

[0327] (1-2-1) Retention and peeling performance of small-sized chip components

[0328] For the adhesive tape obtained in Examples 1, 15 to 23, the obtained adhesive tape was bonded to the surface of the Si chip side of a wafer on which 10 small-sized Si chips (30 μm×40 μm square, thickness 10 μm) were arranged. Then, the Si chip was arranged on the adhesive tape by peeling off the wafer. A semiconductor solid-state laser was used to irradiate each Si chip with a 365 nm laser having an output power of 4 W and 4 kHz from the substrate side of the adhesive tape to peel the Si chip from the adhesive tape.

[0329] The case where all Si chips can be configured on the adhesive tape from the wafer is marked as "○", the case where 8 to 9 Si chips can be configured on the adhesive tape is marked as "△", and the case where less than 7 Si chips can be configured on the adhesive tape is marked as "×" to evaluate the retention performance of the chip components.

[0330] The peeling performance of the chip components (small chips) was evaluated by setting the case where all 10 Si chips could be peeled off as "◎", the case where 8 to 9 Si chips could be peeled off as "○", and the case where 7 or less Si chips could be peeled off as "×". In the case where the adhesive tape has a second adhesive layer, the evaluation was performed in a state where the second adhesive layer was attached to a glass support having a thickness of 2 mm.

[0331] (1-2-2) Residual adhesive on small chip components

[0332] After evaluating the holding performance and peeling performance of small-sized chip components, the surface of the Si chip peeled from the adhesive tape was observed under a microscope to confirm whether there was residual adhesive. The case where there was no residual adhesive was set as "◎", the case where less than 20% of the surface area of ​​the chip component had residual adhesive was set as "0", and the case where more than 20% of the surface area of ​​the chip component had residual adhesive was set as "×" to evaluate the residual adhesive.

[0333] (1-2-3) Peeling off from glass support

[0334] After evaluating the holding performance and peeling performance of the small-sized chip components for Examples 19 to 21, the interface between the adhesive tape and the glass support was observed with a microscope to confirm whether the second adhesive layer was peeled off from the support. The case of no peeling was set as "0", and the case of peeling was set as "×" to evaluate the peeling from the support.

[0335] (2) Measurement of 180° Adhesion Strength and Evaluation of End Lifting

[0336] This evaluation was performed only on the adhesive tapes obtained in Examples 5, 6, 8, 12, 13 and 14.

[0337] Using Autograph (manufactured by Shimadzu Corporation), a peel test was performed in accordance with JIS Z0237 at a temperature of 23°C and a relative humidity of 50% at a tensile speed of 300 mm / min in a 180° direction to measure the 180° adhesive force (N / 25 mm). The 180° adhesive force between the substrate and the ablative layer and the 180° adhesive force between the ablative layer and the barrier layer were measured.

[0338] In addition, a roll of an adhesive tape having a width of 1000 mm and a length of 20 m was prepared in the same manner as in each example. The roll was cut (slit) in the length direction so as to have a tape width of 300 mm. The floating (end floating) between the substrate and the barrier layer at the end (cut surface) of the cut adhesive tape was observed using an optical microscope (manufactured by KEYENCE). The case where no end floating was observed was marked as "○", and the case where one or more end floating was observed was marked as "×", and the end floating was evaluated.

[0339]

[0340]

[0341]

[0342] Industrial Applicability

[0343] According to the present invention, it is possible to provide an adhesive tape for semiconductor device manufacturing that is excellent in chip component peeling performance and can suppress adhesive residue on chip components.

[0344] Description of Reference Numerals

[0345] 1 Chip components

[0346] 1a Electrode

[0347] 4 Adhesive layer

[0348] 4a 1st adhesive layer

[0349] 4b Second adhesive layer

[0350] 5. Substrate

[0351] 7. Driving circuit board

[0352] 7a Electrode

[0353] 8 Laser irradiation device

[0354] 8a Laser

[0355] 9 Laminated body of substrate and adhesive layer

[0356] 10 Ablation layer

[0357] 11 Barrier layer

[0358] 12 Adhesive tape for semiconductor device manufacturing

Claims

1. An adhesive tape for semiconductor device manufacturing, characterized in that: The invention comprises a substrate, an ablation layer, a barrier layer and a first adhesive layer in sequence, The ablation layer is a layer that is deformed by ablation when irradiated with laser light. deformation of the portion of the ablation layer irradiated with the laser beam is transmitted to the barrier layer and the first adhesive layer, The thickness of the barrier layer is less than 25 μm, The adhesive tape for manufacturing a semiconductor device is used for manufacturing a semiconductor device including a step of irradiating a laser beam.

2. The adhesive tape for semiconductor device manufacturing according to claim 1, wherein: The substrate is a resin film.

3. The adhesive tape for semiconductor device manufacturing according to claim 2, wherein: The resin film is a polyester film.

4. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The ultraviolet absorption rate of the ablation layer at a wavelength of 365nm is above 90%.

5. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The storage modulus G' of the ablation layer at 23°C is 1×10 4 Pa or more and 2×10 5 Below Pa.

6. The adhesive tape for semiconductor device manufacturing according to claim 1, wherein: The thickness of the barrier layer is less than 6 μm.

7. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The barrier layer is a polyester film.

8. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The barrier layer has an adhesive resin layer on a surface in contact with the first pressure-sensitive adhesive layer.

9. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The first adhesive layer has a breaking strength of 1 MPa or more.

10. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The storage modulus G' of the first adhesive layer at 23°C is 1×10 4 Pa or more and 2×10 5 Below Pa.

11. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The first adhesive layer contains an ABA type block copolymer.

12. The adhesive tape for semiconductor device manufacturing according to claim 11, wherein: In the ABA type block copolymer, block A contains a structure derived from an aromatic vinyl monomer, and block B contains a structure derived from a (meth)acrylic monomer.

13. The adhesive tape for manufacturing a semiconductor device according to claim 11, wherein: The block B has a structure derived from a monomer having a crosslinkable functional group.

14. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The first pressure-sensitive adhesive layer has a gel fraction of 70% by weight or more and 95% by weight or less.

15. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The first adhesive layer has a thickness of 5 μm or more and 30 μm or less.

16. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The pressure-sensitive adhesive tape for semiconductor device manufacturing has a rolling ball tack of No. 5 or more.

17. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The surface release strength of the first pressure-sensitive adhesive layer of the pressure-sensitive adhesive tape for manufacturing a semiconductor device is 1 MPa or less.

18. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The adhesion between the substrate and the ablation layer is greater than 6N / 25mm.

19. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The adhesion between the ablation layer and the barrier layer is greater than 6N / 25mm.

20. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The first adhesive layer is a curable adhesive layer.

21. The adhesive tape for semiconductor device manufacturing according to claim 1, 2 or 3, characterized in that: The adhesive tape for manufacturing a semiconductor device further comprises a second adhesive layer, and thus the adhesive tape comprises the second adhesive layer, the substrate, the ablation layer, the barrier layer, and the first adhesive layer in this order.